Waste cooking oil (WCO) recycled asphalt is facing issues regarding insufficient thermal oxidation stability and aging resistance. In this research, glycerol esterification was adopted to pretreat WCO, and the consequences of this treatment on the aging resistance and thermal stability of WCO were analyzed. The impacts of varying levels of esterification of WCO on the high-temperature, low-temperature performances, fatigue properties, and aging resistance of recycled asphalt were investigated. Furthermore, the mechanisms of regeneration and the anti-aging of deeply esterified WCO recycled asphalt were revealed by Fourier transform infrared spectroscopy (FTIR) and gel permeation chromatography (GPC) tests. The results indicated that variations in the physical properties of WCO during the aging process were reduced, and its aging resistance was improved following glycerol esterification therapy. The initial thermal decomposition temperature was increased by approximately 115 °C, which resulted in the enhancement of thermal stability significantly. Recycled asphalt obtained from deeply esterified WCO exhibited superior high-temperature, low-temperature performances, and fatigue properties. Moreover, the thermal oxidation stability and aging resistance of recycled asphalt with deep-esterified WCO could be promoted by reducing the oxidation and volatilization of light components during the aging process, with the complex modulus ageing resistance index decreasing by 13.27% and the phase angle ageing resistance index increasing by 14.71%.
Pre-treated waste cooking oil (WCO) and organic montmorillonite (OMMT) were employed for the recycling of aged asphalt, which resulted in the improvement of the design of WCO asphalt rejuvenators and the enhancement of high-temperature performance of WCO-recycled asphalt. The effect of the rejuvenator and the properties of recycled asphalt were evaluated by viscosity, dynamic shear rheometer (DSR), bending beam rheometer (BBR) and scanning electron microscopy (SEM), Fourier-transform infrared spectroscopy (FTIR), and gel permeation chromatography (GPC) tests. The results indicated that aged asphalt could be obviously softened and restored to the level of original asphalt by adding 6% WCO. However, the high-temperature properties of recycled asphalt would be declined by adding too large a dose of WCO rejuvenator. The high-temperature performance of recycled asphalt was significantly improved by the WCO-OMMT complex rejuvenator, and the viscosity and rutting factor of recycled asphalt were increased. Light components of aged asphalt could be supplemented by WCO of the complex rejuvenator. The volatilization of small molecules could be slowed down by the peel structure formed by OMMT and small molecules of the asphalt, which resulted in the proportion of small molecular substances (SMS) being increased by 4% and improvement of the colloidal structure of aged asphalt. The high-temperature and low-temperature performance of recycled asphalt can be improved concurrently by the combination of 6% WCO and 1% OMMT, and this was evidenced by the fact that the high-temperature and low-temperature PG were all upgraded by one level.
Waste cooking oil (WCO) recycled asphalt is facing issues regarding insufficient thermal oxidation stability and aging resistance. In this research, glycerol esterification was adopted to pretreat WCO, and the consequences of this treatment on the aging resistance and thermal stability of WCO were analyzed. The impacts of varying levels of esterification of WCO on the high-temperature, low-temperature performances, fatigue properties, as well as aging resistance of recycled asphalt were investigated. Furthermore, the mechanisms of regeneration and anti-aging of deeply esterified WCO recycled asphalt were revealed by Fourier transform infrared spectroscopy (FTIR) and gel permeation chromatography (GPC) tests. The results indicated that variations in the physical properties of WCO during the aging process were reduced, and its aging resistance was improved following glycerol esterification therapy. The initial thermal decomposition temperature was increased by approximately 115°C, which resulted in the enhancement of thermal stability significantly. Recycled asphalt obtained from deeply esterified WCO exhibited superior high-temperature, low-temperature performances and fatigue properties. Moreover, the thermal oxidation stability and aging resistance of recycled asphalt with deep-esterified WCO could be promoted by reducing the oxidation and volatilization of light components during the aging process.