Butt joints of A5052 aluminum alloy and SS400 steel, with a new type of chamfered edge, are welded by means of metal inert gas welding and ER4043 Al-Si filler metal. The microhardness and microstructure of the joint are investigated. An intermetallic layer is found on the surface of the welding seam and SS400 steel sheet. The hardness of the intermetallic layer is examined using the Vickers hardness test. The average hardness values at the Intermetallic (IMC) layer zone and without the IMC layer zone were higher than that of the welding wire ER4043. The tensile strength test showed a fracture at the intermetallic layer when the tensile strength is 225.9 MPa. The tensile value test indicated the average of welds was equivalent to the 85% tensile strength of the A5052 aluminum alloy. The thickness of the intermetallic layers is non-uniform at different positions with the ranges from 1.95 to 5 μm. The quality of the butt joint is better if the intermetallic layer is minimized. The Si crystals which appeared at the welding seam, indicating that this element participated actively during the welding process, also contributed to the IMC layer’s formation.
The tungsten inert gas (TIG) welding method most commonly used to weld ferrous metals, nonferrous metals, and other metals since it is simple, easily implemented, and achieves consistent high-quality welds. In this study, butt joints produced between aluminum alloy A6061-T6 and stainless steel SUS304L have been achieved by using TIG welding with ER4047 filler metal. The macrostructure and microstructure of the resulting specimens were analyzed by means of an optical microscope (OM), a scanning electron microscope (SEM), and an energy dispersive X-ray spectrometer (EDS). A uniform intermetallic layer was found at the interface between the stainless steel and the weld seam having a thickness of 2 µm, and the intermetallic compound (IMC) includes Fe4Al13, Fe2Al5, and FeAl3 phases. The micro-hardness and tensile strength of the weld joints were also investigated. Due to Si content in the compensating metal, there was a prevention of iron diffusion into the aluminum, thus hindering the development of the IMC layer and reducing its thickness in such a way that the weld joint strength increases. The analyzed results show that the average micro-hardness of the stainless steel, weld seam, aluminum alloys, and IMC layer were 218 HV, 88.3 HV, 63.3 HV, and 411 HV, respectively. The fracture occurred at the brazed interface, and the ultimate tensile strength value reached 225 MPa.
In metal cutting, surface roughness plays an important role in assessing the quality of processed products. The roughness depends greatly on the selection of machining parameters such as cooling conditions and cutting parameters. For this purpose, cooling conditions including dry, MQL, and Silica-based nanofluid MQL as well as cutting parameters including cutting speed, depth-of-cut and feed-rate were investigated to determine their influence on machining roughness during hard milling of AISI H13 steel. The DOE method developed by G. Taguchi was used to design the experiments. An analysis of the signal-to-noise response and ANOVA were carried to obtain the optimal values of cutting parameters for minimizing surface roughness. The results of the present study show that Silica-based nanofluid MQL, minimum feed-rate, minimum depth-of-cut, and maximum cutting speed is an optimal cutting condition for reducing machining roughness.
In manufacturing practice, manufacturers always strive to achieve both quality and productivity targets simultaneously. In the first part, this study examines the relationship between input factors, including cutting speed, depth of cut, and feed rate, and the output response, which is surface roughness, when milling hardened SKD11 alloy steel under minimum coolant lubrication conditions using SiO2 nanofluid. The input parameters are divided into four levels to determine their influence on surface roughness and to find the optimal conditions for achieving the minimum surface roughness. The experimental design was conducted using an L16 array. A second-order regression model was developed to describe the relationship between the input variables and the output response. In the second part, multi-objective optimization was performed to simultaneously achieve the minimum surface roughness and the maximum material removal rate (MRR). The Response Surface Methodology (RSM) was employed in this study. The results indicated that to achieve the minimum surface roughness, machining should be performed at a cutting speed of 100 m/min, a cutting depth of 0.2 mm, and a feed rate of 0.01 mm/tooth. With these settings, the predicted surface roughness could reach 0.0451 µm. On the other hand, for the multi-objective optimization, to achieve the minimum surface roughness and the maximum MRR simultaneously, machining should be carried out at a cutting speed of 100 m/min, a cutting depth of 0.36 mm, and a feed rate of 0.0168 mm/tooth. With this cutting condition, the predicted surface roughness could reach 0.1069 µm, and the predicted MRR could reach 775.06 mm3/min