Vitreous SiO2 thin films thermally grown onto Si wafers were bombarded by Au ions with energies from 0.005 to 11.1 MeV/u and by ions at constant velocity (0.1 MeV/u A197u, T130e, A75s, S32, and F19). Subsequent chemical etching produced conical holes in the films with apertures from a few tens to ∼150 nm. The diameter and the cone angle of the holes were determined as a function of energy loss of the ions. Preferential track etching requires a critical electronic stopping power Seth∼2 keV/nm, independent of the value of the nuclear stopping. However, homogeneous etching, characterized by small cone opening angles and narrow distributions of pore sizes and associated with a continuous trail of critical damage, is only reached for Se>4 keV/nm. The evolution of the etched-track dimensions as a function of specific energy (or electronic stopping force) can be described by the inelastic thermal spike model, assuming that the etchable track results from the quenching of a zone which contains sufficient energy for melting. The model correctly predicts the threshold for the appearance of track etching Seth if the radius of the molten region has at least 1.6 nm. Homogeneous etching comes out only for latent track radii larger than 3 nm.
We show direct experimental evidence that radiation effects produced by single MeV heavy ions on a polymer surface are weakened when the length of the ion track in the material is confined into layers of a few tens of nanometers. Deviation from the bulk (thick film) behavior of ion-induced craters starts at a critical thickness as large as , due to suppression of long-range additive effects of excited atoms along the track. Good agreement was found between the experimental results, molecular dynamic simulations, and an analytical model.
Features produced by swift heavy ions on polymer thin films at different temperatures are used to identify the transition between vitreous and viscoelastic behaviors (the glass transition temperature) and to probe the relaxation of nanodeformations in the material. Scanning force microscopy images reveal nanometer-sized craters and raised regions around the point of ion impact. The size of such defects is independent of temperature for but above a critical temperature crater dimensions increase steeply and no plastic deformation is observed. This critical temperature is sensitive to the cooling rate, and for rapidly cooled targets it is close to the glass transition temperature of the polymer.
Aluminum oxide films deposited on silicon by atomic layer chemical vapor deposition were annealed in an -enriched oxygen atmosphere under various conditions of temperature, time, and pressure. Cavity formation at the film surface was monitored by atomic force microscopy and it was seen to depend on annealing parameters. Areal densities and profiles of oxygen incorporated from the gas phase were determined by nuclear reaction techniques. A propagating front of incorporated oxygen from the gas/solid interface toward the film/substrate interface was observed. This was modeled as a diffusion-reaction process, where isotopic exchange is the reaction channel. The model is capable of reproducing the observed profiles and areal densities as well as their dependence on annealing parameters.
1 May 2003 in Nuclear Instruments and Methods in Physics Research Section B: Beam Interactions with Materials and Atoms