In this study, a new technical process for hardening wood fiber insulation boards is introduced. During the dry-process, the fibers are usually glued with polymeric-diphenylmethane-diisocyanate (pMDI) and hardened to wood fiber insulation boards using a steam-air mixture. However, the maximum temperature reached in the steam-air process was 100 °C, and it was impossible to use an alternative binding agent for the gluing of the wood fiber insulation boards other than pMDI. When incubated with laccase-mediator-system (LMS) as a naturally based bonding system, temperatures of over 120 °C are required because of the chemical wood composition, especially the lignin. In this case, the hot-air/hot-steam process offers new technical opportunities for realizing temperatures above 100 °C. In this study, wood fiber insulation boards were glued with LMS, vs. reference boards with inactivated LMS, laccase alone, and 4% pMDI. Then, the boards were hardened using one of three processes: with steam-air mixture, with hot-air, and with hot-air/hot-steam. Through the hot-air/hot-steam process, temperatures of well over 120 °C were attainable. All the insulation boards hardened using the hot-air/hot-steam process showed better physical and technical properties than those hardened with steam-air mixture or hot-air alone. The reason for this is a sudden increase of temperature after the adding of steam because high temperatures insure that the LMS activated wood fiber surface lignins are completely plasticized. As a result the physical-technological properties such as internal bond strength, compression strength, and short term water absorption of insulation boards treated with LMS were comparable to those boards treated with 4% pMDI.
In this work, the results of the enzymatic oxidation of TMP-fibers (thermomechanical pulp) and a well-structured lignin model compound, the dehydropolymer (DHP), were investigated by different 14C and 13C methods, caused by a Laccase–Mediator-System (LMS). These methods are the nuclear magnetic resonance spectroscopy (13C-NMR) with DHP (unmarked) and the determination of the 14CO2 release of 14C-marked DHP and TMP-fibers. The 13C-NMR measurements were chosen to analyze the structural changes of the LMS-treated DHP model compounds and TMP-fibers qualitatively and quantitatively. The data of 14CO2 release give an explanation of the demethylation of DHP and TMP-fibers. The effect of the LMS is shown by comparing the results in respect of DHP and TMP-fibers, which were only treated with laccase and of an inactivated LMS as the control. Comparing the results of the 13C-NMR method, in particular the use of the Mediator during the enzymatical treatment, showed significant changes in the structure of the DHP. Also, the TMP-fibers were materially influenced by the LMS. The analysis of the 14CO2 release data of the 14C-marked DHP and TMP-fibers revealed that the rate of 14CO2 increases in the 14C-2 atom as well as in the O14CH3 group within the first hour of Laccase–Mediator incubation. Therefore, the 14CO2 release from the DHP was higher than from the TMP-fibers.
The thermal insulation of buildings using wood fiber insulation boards (WFIBs) constitutes a positive contribution towards climate change. Thereby, the bonding of wood fibers using mainly petrochemical-based resins such as polymeric diphenylmethane diisocyanate (pMDI) is an important measure to meet required board properties. Still there is a need to reduce or partial substitute the amount of these kinds of resins in favor of a greener product. This study therefore focusses on the feasibility of reducing the amount of pMDI by 50% through the addition of 1% BioPiva 395 or Indulin as two types of softwood Kraft-Lignin and lignin rich canola hulls together with propylene carbonate as a diluent. A panel density of 160 kg/m3 and a thickness of 40 mm was aimed. The curing of these modified pMDI was investigated by using two types of techniques: hot-steam (HS) and innovative hot-air/hot-steam-process (HA/HS). The WFIBs were then tested on their physical-mechanical properties. The equilibrium moisture content (EMC) was determined at two different climates. An exemplary investigation of thermal conductivity was conducted as well. The WFIBs did undergo a further chemically based analysis towards extractives content and elemental (C, N) composition. The results show that it is feasible to produce WFIBs with lower quantities of pMDI resin and added lignin with enhanced physical-mechanical board properties, which were lacking no disadvantages towards thermal conductivity or behavior towards moisture, especially when cured via HA/HS-process.
An albumin adhesive derived from animal blood was used for the first time for the production of two kinds of fiberboard in a dry process: medium-density fiberboard (MDF) and wood fiber insulation board (WFI). Additionally, the curing for WFI was completed using an innovative hot-air/hot-steam (HA/HS) process. There is a general importance to develop alternatives to substitute common binding agents, such as urea-formaldehyde (UF) or polymeric methylene diphenylene diisocyanate (pMDI) resins, and to develop value-added opportunities for such waste material from slaughterhouses. An adhesive analysis was performed to understand the curing reaction of these protein adhesives, which showed good properties in regards to viscosity or gel time. The physical-mechanical results showed on the one hand that the albumin adhesive could compete with UF-bonded MDF regarding tensile strength and modulus of rupture in conformity to the European Standard, but it failed to meet requirements for thickness swelling. The albumin adhesive also can compete with pMDI bonded WFI regarding tensile and compression strength, but it showed non-viable results for short-term water absorption.