Achieving and predicting long-term durability for reinforced concrete structures particularly in marine environments remains a matter of much interest. Recent research findings based on observations from actual bridge performance and specially conducted long-term experiments for a wide variety of concretes indicate that chloride concentrations are involved only indirectly in initiating reinforcement corrosion and in serious active corrosion. For high quality concretes the critical aspect for long-term durability is the loss of concrete alkalinity, i.e. the acid neutralising capacity of the concrete, principally imparted by its cement content. Alkalinity is reduced, normally very slowly, by the rate of dissolution of calcium hydroxide. However, it is increased by chlorides. It is also increased by a greater internal surface area available for dissolution, such as in poor quality, porous, concretes. Only when the concrete pH drops sufficiently, to a level set by chemical thermodynamic conditions, will large-scale reinforcement corrosion be possible. Importantly, cracking of concrete cover through to the reinforcing bars is likely to cause accelerated localised loss of alkalinity, and thus severe very localised corrosion. Several examples of this are given, drawn from practical reinforced concrete structures. These observations have serious implications for serviceability inspections and for predicting remaining structural life.
Even in harsh marine environments, concrete structures reinforced with steel can show excellent long-term durability, with little or no reinforcement corrosion. Very few actual reinforced concrete (RC) structures have been closely scrutinized over many years and subject to interpretation using recent state-of-the-art understanding gained from detailed laboratory observations. Such a case is described for an 80-year-old RC structure observed annually over about 30 years in what is essentially an extraordinary long experiment. Despite very high chloride concentrations, field excavation evidence showed that reinforcement corrosion overall remains minimal, except where insufficient concrete compaction permitted air-voids to initiate quite severe, very localized corrosion even with still high concrete pH. It is possible that the use of blast furnace slag as aggregate may have assisted the observed durability. The case study supports other studies that show that it is possible to achieve long-term durable and therefore sustainable RC structures without additives and using only conventional reinforcement steels and conventional cements and aggregates. However, the potential dangers of deep narrow cracking extending to the reinforcement and the potentially deleterious effects of alkali–aggregate reactivity of some aggregates needs to be considered.
The critical role of manganese sulphide (MnS) inclusions for the initiation of the short-term growth of pitting or localized corrosion of low carbon steels has long been recognized. Classical results show that pitting probability and pitting severity increases with increased sulphide concentration for low carbon steels as a result of magnesium sulphides acting as local cathodes for initiating pitting corrosion. However, the iron carbides (cementite) in steels can also act as local cathodes for initiation of pitting corrosion. Herein it is proposed that there is competition between pits for cathodic area and that this will determine the severity of pitting and general corrosion observed in extended exposures. Preliminary experimental data for immersion exposures of up to 56 days in natural seawater of three low carbon steels show, contrary to conventional wisdom, greater pit depths for the steels with lower S content. However, the pit depth results are consistent with lower C/S ratios. This is considered to support the concept of cathodic competition between C and S. It is proposed that this offers explanations for a number of other phenomena, including the thus far unexplained apparently higher reactivity of some MnS inclusions.
An important structural component for cavity brick and masonry-veneer construction are wall ties. Typically, they are galvanized steel, sufficiently strong to provide continuity for transmission of direct and shear forces. However, field observations show they are prone to long-term corrosion and this can have serious structural implications under extreme events such as earthquakes. Opportunistic observations show corrosion occurs largely to the internal masonry interface zone even though conventional Code requirements specify corrosion testing for the whole tie. To throw light on the issue electrochemical test for 2 grades of galvanized ties and 316 stainless steels combined with three different mortar compositions are reported. Most severe corrosion occurred at the masonry interface and sometimes within the masonry itself. Structural capacity tests showed galvanized ties performed better than stainless steel ties in lieu of stainless steel R4 class ties presenting significantly greater relative losses of yield strength, ultimate tensile strength and elongation structural capacity compared to R2 low galvanized and R3 heavy galvanized tie classes.
The present paper reports on four-year field investigations aimed at ascertaining internal corrosion rates for offshore wind-power generation monopiles, despite these being designed to obviate internal corrosion through oxygen exclusion. Results for mild steel strips within the enclosed, quiescent, uPVC simulated seawater environments are presented as a function of relative to mean tide level, period of exposure and localised pollution of seawater. Detailed pit depth measurements are also reported for various exposure periods, with the magnitude of such corrosion displaying a bi-modal behaviour as a function of exposure time, consistent with much other data. No evidence was found of the classical corrosion profile for vertical steel structures (e.g. piles) or of accelerated low water corrosion usually associated with microbiologically influenced corrosion caused by elevated seawater nutrient concentrations. It is proposed that the observed corrosion behaviours primarily are the result of the shielded quiescent environment. The practical implications are briefly discussed.
Not counting domestic dwellings, it has been estimated that in Australia alone, some tens of thousands of masonry buildings and structures have exceeded their design life, with many of these being at risk of partial (or worse) collapse from falling or dislodged masonry. This has significant implications for human life but also for the urban environment and economic health of building owners, managers, and insurers and for local and national economies. This risk can mainly be attributed to the slow deterioration of masonry under atmospheric and other environments and the corrosion of so-called wall ties. Wall ties are relatively thin pieces of steel that tie the outer leaf of masonry walls to the stabilized inner leaf. The problem is likely severe for scenarios such as cyclonic and earthquake events, as they cause area-wide damage and the potential wide-spread loss of human life—losses that could be prevented by timely intervention. This paper reports on the in situ inspection of two case study buildings and the data obtained from controlled wall tie corrosion field trials, which are used to develop predictive models of structural response. These models will inform practical tools that will be developed for building assessment, cost-effective monitoring, and rectification, assisting in the management of existing masonry buildings.