This work aims to examine the mechanical and thermal behavior of rising husk fiber/starch reinforced epoxy polymer composites. Experiments are carried out to study the effect of fiber and filler volume percentage on the mechanical, and thermal behavior of epoxy-based polymer composites. The volume of fibre and filler is varied by 10%,20%,30%, 40%, and starch 5% and 10% and 1.5%, respectively. The specimens are fabricated by using hand layup technique. The specimens are expurgated according to ASTM standards. The effects of rising husk fiber and filler were examined under different thermal conditions. The mechanical results show that the addition of fiber increased the impact characters of epoxy resin, whereas the addition of starch shell filler increased the termal conductivity of the composite. We found that the results show that the stacking sequences of rising Husk/starch fibers have a significant impact on thermal conductivity. Composites with the stacking sequence mode RH40 with 15 % starch exhibit the highest thermal conductivity 2.6 W/m·K an enhancement of 472,72% over the thermal conductivity of the PC resin (0.55 W/m·K) it is significant
Polymer-based composites have emerged as viable alternatives to metals for applications requiring reduced weight, corrosion resistance, and cost-effectiveness; however, their relatively low mechanical strength remains a significant limitation. This study evaluates the flexural performance of unsaturated polyester composites reinforced with coconut shell charcoal (CC) powder at filler contents of 0%, 10%, 20%, and 30% by weight, in accordance with ASTM D790. The incorporation of 20 wt% CC yielded the highest flexural strength of 132.43 MPa, representing a 153% improvement compared to pure polyester (52.10 MPa). Flexural modulus also increased substantially at this composition, indicating enhanced stiffness resulting from improved interfacial bonding and efficient stress transfer. In contrast, increasing the filler content beyond 20 wt% resulted in a reduction of up to 32% in strength, attributed to particle agglomeration and void formation. Overall, the results identify 20 wt% CC as the optimal reinforcement level, significantly improving energy absorption and bending resistance, thereby positioning this composite as a promising candidate for lightweight structural applications.
5 October 2023 in The International Journal of Mechanical Engineering and Sciences
The development of polymer composite materials has been widely developed as an alternative material to replace metal materials due to various advantages such as having relatively good mechanical strength, low density, and easy manufacturing process, but polymers have many disadvantages that they easily crack when impacted. One of the most widely used materials for composite matrices is unsaturated polyester polymers which are widely used in vehicle, aircraft, and ship hull components as well as vehicle components. The crack study is important because it causes the material to no longer be able to support loads below its yield strength, therefore causing failure to occur more quickly. One way to overcome material failure due to cracks in composite materials is to prevent crack propagation by adding reinforcing materials. In this study, a composite material was made using rice husk fiber to increase the crack resistance of the polyester composite matrix. From the results of the crack test, it is known that there is a tendency to increase the percentage variable of the addition of rice husk by 5%, 10%, 15%, and 20%. The expected value obtained to determine the crack resistance of the material is the value of the stress intensity factor (K1c). The highest K1c price was obtained at a 15% rice husk percentage variable of 1.558 MPa.m0.5, this price could increase the price of the pure polyester stress intensity factor (K1c) by 0.667 MPa.m0.5, indicating an increase of 233.58%.
The development of environmentally friendly composites from natural fibers is an absolute thing to do to replace non-degradable synthetic composites. Some of the weaknesses of natural fiber composites are low mechanical strength, ease of cracking, no moisture resistance, and high-temperature resistance. One of the things that has been done is to make a combination of synthetic materials as a matrix derived from unsaturated polyester reinforced with natural fibers from crushed rice husk particles and starch from sago flour which is used to reduce the percentage of synthetic materials to be able to form composites that are easily decomposed. From the research, it was found that the strength of crack resistance could be increased with a mixture of polyester reinforced with rice husk fiber and sago flour, obtaining an increase in crack resistance strength until the addition of rice husk with a percentage of 15%. While increasing the RH content above 15%, the crack strength value decreases due to the saturation of the RH molecules in the UP which is no longer bound to the UP molecules. The highest crack strength values occurred for the addition of the percentage of RH and SS to the UP material with the addition of 5% SS, which obtained a cracking force of 550 N while the strength of pure polyester was only 37 N. This shows that RH and SS materials can bond with UP molecules and some molecules of RH and SS can prevent cross-linking of polyester molecules. Meanwhile, the addition of SS up to 10% decreases the fracture force obtained, indicating that not all of the sago starch can bind to the polyester molecules.
31 October 2022 in METAL: Jurnal Sistem Mekanik dan Termal
Unsaturated polyester is a polymer that is widely used as a basic matrix to form strong composites for engineering applications such as for cars, ships and aeroplanes. The advantages of using this material are owing to have a fairly high tensile strength when reinforced with appropriate reinforcing fibers, light and easy to shape. However, due to its brittle nature, this material cannot withstand shock loads. Therefore, it is necessary to overcome that weakness. Crude Palm Oil (CPO) can give benefits as a strengthening agent. However, its proper mixture to polyester need to be figured out so that it would help in improving crack resistance properties of this polyester. This can be done by determining of fracture resistance value of the mixture polymer. A crack resistance testing was carried out and crthe itical stress intensity factor was calculated based on ASTM D 5005. The composition of the CPO mixture was varied from 100%: 0%, 10%: 20%, 30%: 40%. From the test results, it can be identified that the greatest critical stress intensity factor is  = 15.787  MPa.m1/2. This is found out in composition of 30% CPO. Meanwhile the critical intensity factor of pure Unsaturated Polyester (UP) is only 2,023 MPa.m1/2. There is approximately 700% improvement that can be gained in mixing with CPO.
5 November 2025 in Jurnal Engine: Energi, Manufaktur, dan Material
One of the polymer materials widely used as a matrix material in the manufacture of composites is unsaturated polyester, which is widely used in engineering fields such as ships, vehicles and also widely used in engineering fields in general. This polyester material for direct use in the construction field still has low mechanical strength and cannot experience good tensile deformation, and is difficult to experience bending loads and can break if it gets a large amount of flexibility. To increase its bending strength, this polyester material is mixed with reinforcing material from bamboo fibre material, which is first refined with various percentages of the mixture ranging from 10% to 30%. After mixing, flexural testing is carried out by applying a flexural load in the middle of the test sample and both ends of the sample are supported with flexural strength that increases along with the resistance of the test material. From the research for flexural testing, it was found that a polyester polymer mixed with bamboo fiber with a percentage of 20% obtained a maximum flexural stress value of σ = 97.35 MPa. When compared with the value of the pure polyester flexural stress of σ = 37.29 MPa, there was an increase in flexural strength of 261.16%.