The high demand for wood-based composites generates a greater use of wood adhesives. The current industrial challenge is to develop modified synthetic adhesives to remove harmful formaldehyde, and to test natural adhesives. The scope of the current research included the manufacturing of high-density fiberboards (HDF) using natural binders such as polylactic acid (PLA), polycaprolactone (PCL), and thermoplastic starch (TPS) with different resination (12%, 15%, 20%). The HDF with biopolymers was compared to a reference HDF, manufactured following the example of industrial technology, with commonly used adhesives such as urea-formaldehyde (UF) resin. Different mechanical and physical properties were determined, namely modulus of rupture (MOR), modulus of elasticity (MOE), internal bonding strength (IB), thickness swelling (TS), water absorption (WA), surface water absorption (SWA), contact angle, as well as density profile; scanning electron microscope (SEM) analysis was also performed. The results showed that increasing the binder content significantly improved the mechanical properties of the panels in the case of starch binder (MOR from 31.35 N mm−2 to 40.10 N mm−2, IB from 0.24 N mm−2 to 0.39 N mm−2 for dry starch), and reduces these in the case of PLA and PCL. The wet method of starch addition improved the mechanical properties of panels; however, it negatively influenced the reaction of the panels to water (WA 90.3% for dry starch and 105.9% for wet starch after 24 h soaking). Due to dynamically evaporating solvents from the PLA and PCL binding mixtures, a development of the fibers’ resination (blending) techniques should be performed, to avoid the uneven spreading of the binder over the resinated material.
In this research, the assessment of the impact of natural biopolymer binders on selected mechanical and physical properties of lignocellulosic composites manufactured with different resination (12%, 15%, 20%). Different mechanical and physical properties were determined: modulus of rupture, modulus of elasticity, internal bonding strength, thickness swelling, water absorption, contact angle, and density profile. Moreover, thermal properties such as thermogravimetric analysis and differential scanning calorimetry were studied for the polymers. The results showed significant improvement of characterized features of the composites produced using biopolymers. However, the rise of the properties was visible when the binder content raised from 12% to 15%. Further increase of biopolymer binder did not imply a considerable change. The most promising biopolymer within the tested ones seems to be polycaprolactone (PCL).
4 October 2019 in Clean Technologies and Environmental Policy
In this study, layered composites were produced with different biopolymer adhesive layers, including biopolymer polylactic acid (PLA), polycaprolactone (PCL), and biopolymer blends of PLA + polyhydroxybutyrate (PHB) (75:25 w/w ratio) with the addition of 25, 50% microcrystalline cellulose (MCC) and 3% triethyl Citrate (TEC) for these blends, which acted as binders and co-created the five layers in the elaborated composites. Modulus of rupture (MOR), modulus of elasticity (MOE), internal bonding strength (IB), density profile, differential scanning calorimetry (DSC), thermogravimetric analysis (TGA), and scanning electron microscopy (SEM) analysis were obtained. The results showed that among the composites in which two pure biopolymers were used, PLA obtained the best results, while among the produced blends, PLA + PHB, PLA + PHB + 25MCC, and PLA + PHB + 25MCC + 3TEC performed best. The mechanical properties of the composites decreased with increases in the MCC content in blends. Therefore, adding 3% TEC improved the properties of composites made of PLA + PHB + MCC blends.