Tank bio-oxidation is a biohydrometallurgical technology widely used for metal recovery from sulfide concentrates. Since carbon availability is one of the key factors affecting microbial communities, it may also determine the rate of sulfide concentrate bio-oxidation. The goal of the present work was to evaluate the effect of carbon sources on the bio-oxidation of the concentrate containing 56% pyrite and 14% arsenopyrite at different temperatures (40 and 50 °C) in stirred tank reactors. CO2 was supplied into the pulp of the first reactor (about 0.01 L/min) and 0.02% (w/v) molasses was added to the pulp of the second one, and no additional carbon sources were used in the control tests. At 40 °C, 77% of pyrite and 98% of arsenopyrite were oxidized in the first reactor, in the second one, 73% of pyrite and 98% of arsenopyrite were oxidized, while in the control reactor, 27% pyrite and 93% arsenopyrite were oxidized. At 50 °C, in the first reactor, 94% of pyrite and 99% of arsenopyrite were oxidized, in the second one, 21% of pyrite and 94% of arsenopyrite were oxidized, while in the control reactor, 10% pyrite and 92% arsenopyrite were oxidized. The analysis of the microbial populations in the reactors revealed differences in the total number of microorganisms and their species composition. Thus, it was shown that the use of various carbon sources made it possible to increase the intensity of the concentrate bio-oxidation, since it affected microbial populations performing the process.
The aim of the present work was to perform copper, nickel, and platinum group metals (PGMs) recovery from low-grade copper–nickel concentrate containing pyrrhotite, pentlandite, and chalcopyrite by bioleaching in stirred tank reactors in batch mode and subsequent cyanidation. The concentrate contained (%) Fe 32.7, Cu 0.7, Ni 2.3, Stotal 20.9, Ssulfide 17, 0.1 g/t Pt, and 1.35 g/t Pd. The bioleaching was performed at 30 and 40 °C using two different microbial consortia. At 30 °C, bioleaching was performed using mixed culture including Acidithiobacillus ferrivorans strains isolated from the sample of acid mine drainage from copper–nickel deposit. At 40 °C, bioleaching was performed using microbial population formed during long-term bioleaching of copper-zinc concentrate at 40 °C. Bioleaching was performed for 40 days at pulp density of 10% (solid to liquid ratio 1:10). At 30 °C, 70% Ni and 14% Cu were leached, while 72% Ni and 34% Cu were recovered in the solution at 40 °C. PGM were extracted from the concentrate and bioleaching residue obtained at 40 °C by cyanidation. Cyanidation made it possible to extract 5.5% Pt and 17.3% Pd from the concentrate and 37.8% Pt and 87.8% Pd from the bioleaching residue. Thus, it was shown that the concentrate studied might be processed using bioleaching and subsequent cyanidation to extract both non-ferrous metals and PGM.
Bioleaching may be effectively used to extract nonferrous metals from sulfide ores and concentrates. At the same time, some minerals are refractory and their bioleaching rate is often comparatively low that does not allow the required metal extraction rate to be achieved. In the present work, we studied the two-stage process, which included stages of biological and chemical leaching, to improve copper extraction from low grade Cu–Zn sulfide concentrate containing chalcopyrite, tennantite, pyrite, and sphalerite. Bioleaching was conducted in the continuous mode in three laboratory scale reactors connected in series. The pulp density was 10% and the residence time was 7 days. The temperature was 40 °C in the 1st reactor and 50 °C in the 2nd and 3rd reactors. Bioleaching allowed the extraction of 29.5 and 78% of Cu and Zn, respectively. The solid bioleach residue obtained was then treated for additional Cu and Zn recovery using high temperature leaching at 90 °C for 25 h. The liquid phase of the bioleaching pulp contained Fe3+ ions, which is the strong oxidant, and the leach solution was supplemented with NaCl. In the presence of the maximal NaCl concentration (1 M), Cu and Zn extraction reached 48 and 84%. Thus, two-stage leaching may allow to increase bioleaching efficiency and may be used to improve the bioleaching rate of refractory minerals, such as chalcopyrite.
In the present study, the effect of additional carbon sources (carbon dioxide and molasses) on the bio-oxidation of a pyrite–arsenopyrite concentrate at temperatures of 40–50 °C was studied, and novel data regarding the patterns of the bio-oxidation of gold-bearing sulfide concentrates and the composition of the microbial populations performing these processes were obtained. At 40 °C, additional carbon sources did not affect the bio-oxidation efficiency. At the same time, the application of additional carbon dioxide improved the bio-oxidation performance at temperatures of 45 and 50 °C and made it possible to avoid the inhibition of bio-oxidation due to an increase in the temperature. Therefore, the use of additional carbon dioxide may be proposed to prevent the negative effect of an increase in temperature on the bio-oxidation of sulfide concentrates. 16S rRNA gene profiling revealed archaea of the family Thermoplasmataceae (Acidiplasma, Ferroplasma, Cuniculiplasma, and A-plasma group) and bacteria of the genera Leptospirillum, with Sulfobacillus and Acidithiobacillus among the dominant groups in the community. Temperature influenced the composition of the communities to a greater extent than the additional sources of carbon and the mode of operation of the bioreactor. Elevating the temperature from 40 °C to 50 °C resulted in increases in the shares of Acidiplasma and Sulfobacillus and decreases in the relative abundances of Ferroplasma, Leptospirillum, and Acidithiobacillus, while Cuniculiplasma and A-plasma were more abundant at 45 °C. A metagenomic analysis of the studied population made it possible to characterize novel archaea belonging to an uncultivated, poorly-studied group of Thermoplasmatales which potentially plays an important role in the bio-oxidation process. Based on an analysis of the complete genome, we propose describing the novel species and novel genus as “Candidatus Carboxiplasma ferriphilum” gen. nov., spec. nov.
In the present work the effect of alkaline sulfide leaching (ASL) on the extraction of copper and zinc from low-grade copper concentrate containing chalcopyrite, tennantite, sphalerite, and pyrite during batch and continuous bioleaching experiments was studied. It was demonstrated that ASL and further bioleaching may be a promising approach for treatment of copper–zinc concentrates containing tennantite as this approach allows increasing copper extraction degree in comparison to one-stage bioleaching by 1.6–2.3 times. Thus, ASL was shown to be effective for pretreatment of tennantite containing concentrates to improve bioleaching for copper extraction. At the same time, ASL led to decrease in zinc extraction by 1.4–1.5 times. Therefore, the development of combined hydrometallurgical processes including ASL and bioleaching for effective metal leaching requires further studies to avoid negative effect on zinc extraction.
Microbially assisted bio-oxidation of sulfide concentrates in stirred-tank reactors (stirred-tank reactor bio-oxidation (STRB)) and acid pressure oxidation (POX) are widely used to pretreat refractory sulfide concentrates and increase gold extraction via cyanidation. Continuous STRB requires a comparatively long residence time; however, in some cases, it cannot effectively oxidize some sulfide minerals. POX enables oxidation in a short residence time. At the same time, if a processed concentrate contains a large amount of sulfur, it decreases the ratio of the solid mineral phase to liquid (pulp density) during POX and limits its economic attractiveness. In the present work, experiments were performed to investigate the problems associated with both processing methods for refractory sulfide concentrates. The experiments combined both treatments (STRB and POX) based on the example of a pyrite–arsenopyrite gold-bearing concentrate. The gold recovery from the untreated concentrate via cyanidation reached 58%. Continuous STRB for 2, 4, and 6 days oxidized 43, 74, and 79% of the sulfide sulfur (Ss), respectively. The gold recovery rates from the bio-oxidation residues were 68, 82, and 88%, respectively. The pressure oxidation of both the concentrate and STRB residues increased Ss oxidation by 97–99% and gold recovery by 96–97%. For 2 days, STRB decreased the Ss content and increased the possible liquid-to-solid ratio for POX. The combined processes result in a new promising direction because the POX stage allows high gold recovery, whereas combining STRB and POX provides products for further POX in terms of Ss content and increases POX productivity.