A bulk scale process is implemented for the production of nanostructured film composites comprising unary or multi-component metal oxide nanoparticles dispersed in a suitable polymer matrix. The as-received nanoparticles, namely Al $$_2$$ O $$_3$$ , SiO $$_2$$ and TiO $$_2$$ and binary combinations, are treated following specific chemical and mechanical processes in order to be suspended at the optimal size and composition. Subsequently, a polymer extrusion technique is employed for the fabrication of each film, while the molten polymer is mixed with the treated metal oxide nanoparticles. Transmission and reflection measurements are performed in order to map the optical properties of the fabricated, nanostructured films in the UV, VIS and IR. The results substantiate the capability of the overall methodology to regulate the optical properties of the films depending on the type of nanoparticle formation which can be adjusted both in size and composition.
Nanocomposite polymer films are a very diverse research field due to their many applications. The search for low-cost, versatile methods, producing regulated properties of the final products, has thus become extremely relevant. We have previously reported a bulk-scale process, dispersing granulated metal oxide nanoparticles, of both unary and multi-component nature, in a low-density polyethylene (LDPE) polymer matrix, establishing a reference in the produced films’ optical properties, due to the high degree of homogeneity and preservation of the primary particle size allowed by this method. In this work, unmodified, free-standing particles, namely zinc oxide (), titanium dioxide (), aluminum oxide (), and silicon dioxide () are blended directly with LDPE, and the optical properties of the fabricated films are compared to those of films made using the granulation process. The direct blending process evidently allows for control of the secondary particle size and ensures a homogeneous dispersion of the particles, albeit to a lesser extent than the granulation process. Despite the secondary particle size being comparatively larger than its granulated counterpart, the process still provides a regulated degree of deagglomeration of the free-standing oxide particles, so it can be used as a low-cost alternative. The regulation of the secondary particle size tunes the transmission and reflection spectra, in both unary and mixed oxide compositions. Finally, the direct blending process exhibits a clear ability to tune the energy band gap in mixed oxides.
We investigate a method for fabricating layers that exhibit both high optical absorption and promising thermoelectric properties. Using plasma-enhanced chemical vapor deposition (PECVD), amorphous Si and Si72Ge28 layers are deposited on glass substrates and subsequently processed via laser annealing to achieve nanostructured layers. Our results show that a single laser annealing pulse at 40 mJ yields the highest power factor, approximately 90 mu W/mK2. Additionally, we observe a maximum absorbance enhancement factor of 60 times in the spectral region near 880 nm for samples treated with a single pulse of 60 mJ compared to untreated samples. The effects of laser energy, the number of pulses, and material choice are further discussed.
This study explores the synthesis of Bismuth Telluride nanoparticles on silicon wafers via spark ablation using metal targets, avoiding toxic or costly precursors. Conducted at room temperature with a direct current arc and an inert gas atmosphere, the process prevents oxidation. The influence of voltage (0.5 kV, 1.0 kV, 1.5 kV), current (3 mA, 6 mA, 10 mA), and gas flow on particle size and distribution was investigated. Optimal conditions were achieved at a gas flow rate of $$2.5\,\hbox {L min}^{-1}$$ , yielding particles sized 10 to 25 nm with a mean diameter of $$17 \pm 3$$ nm, demonstrating tunable synthesis suitable for targeted applications. Graphic abstract
This study presents a comprehensive numerical modeling and performance evaluation of a BaZrS3, perovskite-based, metal-semiconductor-metal (MSM) photodetector using SCAPS-1D, demonstrating its strong potential for high-efficiency photosensing applications. By systematically optimizing the absorber layer's thickness and doping concentration, notable enhancements in responsivity and detectivity were achieved. Under 600 nm irradiation, the photodetector exhibits an impressive responsivity of 0.41 A/W and a high detectivity of 9.87 × 1015 Jones. These findings establish BaZrS3 photo detectors as a promising, cost-effective, and environmentally friendly alternative for next-generation optoelectronic and sensing technologies.