Corrosion is frequently viewed as a catastrophic and unavoidable disaster in marine applications. Every year, a huge cost is incurred on the maintenance and repair of corrosion-affected equipment and machinery. In the marine environment, as-cast nickel–aluminium bronze (NAB) is susceptible to selective phase corrosion. To solve this problem, chromium-reinforced nickel–aluminium bronze was fabricated using the friction stir process (FSP) with improved microstructures and surface properties. A slurry erosion–corrosion test on as-cast and FSPed composites demonstrated that the developed surfaced composite has lower erosion and corrosion rates than the as-cast NAB alloy. The erosion–corrosion rate increased with a decrease in the impact angle from 90° to 30° for both as-cast NAB and prepared composites, exhibiting a shear mode of erosion. The specimens at impact angle 30° experienced more pitting action and higher mass loss compared with those at impact angle 90°. Due to increases in the mechanical properties, the FS-processed composite showed higher erosion resistance than the as-cast NAB alloy. Furthermore, corrosion behaviour was also studied via the static immersion corrosion test and electrochemical measurements under 3.5 wt.% NaCl solution. In a static immersion corrosion test, the FSPed composite outperformed the as-cast NAB composite by a wide margin. The FSPed composite also demonstrated a reduced electrochemical corrosion rate, as revealed by the polarization curve and electrochemical impedance spectroscopic (EIS) data. This reduced rate is attributed to the formation of a Cr oxide film over its surface in the corrosive environment.
13 March 2013 in International Journal of Advanced Materials Manufacturing and Characterization
The present study focuses on fabricating a chromium-reinforced nickel aluminium bronze (NAB) composite using an optimized multi-pass friction stir processing (FSP) technique. The tool rotation, tool traverse speed, and volumetric concentration of the reinforcement were taken as input process parameters, whereas the ultimate tensile strength (UTS), yield strength (YS), percentage elongation (% E), microhardness, and sliding wear rate were taken as output responses. Taguchi-Grey relational analysis (GRA) was utilized for optimizing the input process parameters, which were 1000 r.p.m., 28 mm min−1 and 15.7%, respectively. The most significant parameter was traverse speed, followed by tool rotation and volumetric concentration of the reinforcement. FE-SEM, EDS, and XRD analyses were performed to characterize the as-cast NAB, chromium powder, and FS-processed composite. The tensile strength and wear resistance of the processed composite are enhanced compared to the base NAB alloy on account of significant grain refinement due to the stirring action of the tool pin in the processed zone and the dispersion of chromium reinforcement. The wear rate of the composite was reduced as the tool rotation, traverse speed, and Cr particle volume concentration were increased. The maximum UTS of the prepared composite was 701 MPa, whereas the UTS of the as-cast NAB was 620 MPa. It was observed that as-cast NAB exhibited a hardness value of 286 HV, which was improved to 385 in the FSPed prepared composite. It was found that as-cast NAB exhibited 7.0 × 10–6 gm m−1 of wear rate, whereas the FSPed composite showed a minimum wear rate of 5.5 × 10–6 gm m−1. The microstructural examination revealed that the wear mechanism in the case of as-cast NAB was primarily adhesion, whereas the abrasion was found to be the governing mechanism of material removal in the processed composite.
In this study, Friction Stir Processing (FSP) was applied to produce surface composites of AA2014 by using SiC as a reinforcement. The main aim of the investigation is to study the influence of FSP on the microhardness of AA2014/SiC surface composites. A mathematical model was created by employing the Response Surface Methodology (RSM) to predict the microhardness properties by optimizing FSP parameters like tool rotating speed, tool tilt angle, tool traverse speed, and the number of FSP passes. It was observed that the tool traverse speed of 50 mm min−1, 1000 rpm tool rotating speed, and tool tilt angle of 1° with 2 FSP passes produce surface composites with uniformly dispersed SiC particles. The grain size of the produced surface composites decreased from 26.9 μm in the base matrix to 16.7 μm in the FSPed specimens, enhancing microhardness by 6.25% in the cross-section and 15.36% in the top surface of the FSPed specimens. The dynamic recrystallization and generation of fine-grain microstructure played an essential role in enhancing the microhardness of the material. These results show the effectiveness of the RSM technique in optimizing the FSP parameters and producing the AA2014/SiC for enhanced microhardness applications in aerospace and automobile applications.
In this paper, the effect of tool tilt angle during the Friction Stir Processing was investigated. A tool having a tilt angle of 1˚, 2˚, 3 ˚, and 4˚ were employ