Hybrid mesoporous silica SBA-15, with surface incorporated cross-linked long hydrophobic organic bridges was synthesized using stepwise synthesis. The synthesized materials were characterized by elemental analysis, infrared spectroscopy, nuclear magnetic resonance spectroscopy, nitrogen adsorption, X-rays diffraction, thermogravimetry and scanning and transmission electron microscopy. The functionalized material showed highly ordered mesoporous network with a surface area of 629.0m2g-1. The incorporation of long hydrophobic amine chains on silica surface resulted in high drug loading capacity (21% Mass/Mass) and prolonged release of ibuprofen up till 75.5h. The preliminary investigations suggests that the synthesized materials could be proposed as controlled release devices to prolong the therapeutic effect of short life drugs such as ibuprofen to increase its efficacy and to reduce frequent dosage.
Introduction: Drug delivery systems are the topmost priority to increase drug safety and efficacy. In this study, hybrid porous silicates SBA-15 and its derivatives SBA@N and SBA@3N were synthesized and loaded with an anticancer drug, 5-fluorouracil. The drug release was studied in a simulated physiological environment.Method: These materials were characterized for their textural and physio-chemical properties by scanning electron microscopy (SEM), nuclear magnetic resonance (NMR), Fourier transform infrared spectroscopy (FTIR), small-angle X-ray diffraction (SAX), and nitrogen adsorption/desorption techniques. The surface electrostatics of the materials was measured by zeta potential.Results: The drug loading efficiency of the prepared hybrid materials was about 10%. In vitro drug release profiles were obtained in simulated fluids. Slow drug release kinetics was observed for SBA@3N, which released 7.5% of the entrapped drug in simulated intestinal fluid (SIF, pH 7.2) and 33% in simulated body fluid (SBF, pH 7.2) for 72 h. The material SBA@N presented an initial burst release of 13% in simulated intestinal fluid and 32.6% in simulated gastric fluid (SGF, pH 1.2), while about 70% of the drug was released within the next 72 h. Density functional theory (DFT) calculations have also supported the slow drug release from the SBA@3N material. The release mechanism of the drug from the prepared carriers was studied by first-order, second-order, Korsmeyer–Peppas, Hixson–Crowell, and Higuchi kinetic models. The drug release from these carriers follows Fickian diffusion and zero-order kinetics in SGF and SBF, whereas first-order, non-Fickian diffusion, and case-II transport were observed in SIF.Discussion: Based on these findings, the proposed synthesized hybrid materials may be suggested as a potential drug delivery system for anti-cancer drugs such as 5-fluorouracil.
Background: Chronic wounds continue to be a global concern that demands substantial resources from the healthcare system. The process of cutaneous wound healing is complex, involving inflammation, blood clotting, angiogenesis, migration and remodeling. In the present study, commercially available alginate wound dressings were loaded with heparin. The purpose of the study was to enhance the angiogenic potential of alginate wound dressings and analyze the antibacterial activity, biocompatibility and other relevant properties. We also aimed to conduct some molecular and gene expression studies to elaborate on the mechanisms through which heparin induces angiogenesis. Methods: The physical properties of the hydrogels were evaluated by Fourier transform infrared spectroscopy (FTIR). Swelling ability was measured by soaking hydrogels in the Phosphate buffer at 37 °C, and cell studies were conducted to evaluate the cytotoxicity and biocompatibility of hydrogels in NIH3T3 (fibroblasts). Real-time PCR was conducted to check the molecular mechanisms of heparin/alginate-induced angiogenesis. The physical properties of the hydrogels were evaluated by Fourier transform infrared spectroscopy (FTIR). Results: FTIR confirmed the formation of heparin-loaded alginate wound dressing and the compatibility of both heparin and alginate. Among all, 10 µg/mL concentration of heparin showed the best antibacterial activity against E. coli. The swelling was considerably increased up to 1500% within 1 h. Alamar Blue assay revealed no cytotoxic effect on NIH3T3. Heparin showed good anti-microbial properties and inhibited the growth of E. coli in zones with a diameter of 18 mm. The expression analysis suggested that heparin probably exerts its pro-angiogenetic effect through VEGF and cPGE. Conclusions: We report that heparin-loaded alginate dressings are not cytotoxic and offer increased angiogenic and anti-bacterial potential. The angiogenesis is apparently taken through the VEGF pathway.