This study employed novel joint treatments to strengthen the carbon fiber reinforced polymer (CFRP) composites. Vertically aligned carbon nanotubes (VACNTs) were prepared in situ on the catalyst-treated CF surface via the chemical vapor deposition (CVD) method, intertwining into three-dimensional fiber-nets and fully surrounding CF to form an integrated structure. The resin pre-coating (RPC) technique was further used to guide diluted epoxy resin (without hardener) to flow into nanoscale and submicron spaces to eliminate void defects at the root of VACNTs. Three-point bending testing results showed the “growing CNTs and RPC”-treated CFRP composites yielded the best flexural strength, a 27.1% improvement over the specimens without treatment, while the failure modes indicated that the original delamination failure was changed into “flexural failure” with through-the-thickness crack propagation. In brief, growing VACNTs and RPC on the CF surface enabled toughening of the epoxy adhesive layer, reducing potential void defects and constructing the integrated quasi-Z-directional fiber bridging at the CF/epoxy interface for stronger CFRP composites. Therefore, the joint treatments of growing VACNTs in situ via the CVD method and RPC technique are very effective and have great potential in manufacturing high-strength CFRP composites for aerospace applications.
In this study, anodizing treatment was utilized to etch titanium (Ti) substrates’ surface to prefabricate nano-cavities. Resin pre-coating (RPC) and three silane coupling agents’ coating (CAC) techniques were further applied to porous Ti substrates surface to compare the reinforcement effect of adhesive bonding strength. SEM images show that nano-cavities have been prepared to create a greater contact area and vertical volume on Ti substrate surface, fully covered by resin coatings via RPC. A higher surface roughness and better surface wetting are also obtained by the testing results of atomic force microscope and contact angles. Single lap shear tests results indicate that specimens with “anodizing + RPC” treatment yield the best average shear strength of 20.73 MPa, increased by 31.7% compared to anodizing base strength and at least 63.0% higher than silane KH-550/560/792-coated specimens. A dominant cohesive failure and fiber-tearing on CFRP’s shallow surface, instead of adhesive debonding failure, are shown in the appearances of damaged specimens, proving that the RPC technique has a more effective bonding strength reinforcement in titanium and carbon fiber-reinforced polymer (Ti-CFRP) composites’ toughening. Thus, the simple RPC technique can be regarded as a new-type alternative to adhesive joint toughening to manufacture high-performance composites for aerospace applications.
A shape-controllable laser-engraving treatment (LET) and aramid pulp (AP)-reinforced resin pre-coating (RPC) were used on a titanium (Ti) alloy surface to construct micro-/nano-aramid pulp and epoxy (MAPE) coatings for greater bonding strength with carbon fiber-reinforced polymers (CFRPs). The array pits of regular hexagon on the Ti alloy surface were engraved and vertical spaces between the array pits were created to place the AP-reinforced epoxy for stronger mechanical interlocking. The specimen treated with laser engraving (side length of 0.3 mm) and AP-reinforced RPC yielded the greatest bonding strength of 27.1 MPa, 67.4% higher than the base strength. The failure modes of the Ti-CFRPs composites changed from debonding failure at the Ti/epoxy surface to fiber-damaged failure of the laminated CFRPs panels. The shape-controllable LET and simple AP-reinforced RPC were confirmed as the most feasible and effective combined methods for use on titanium alloy surfaces for manufacturing stronger Ti-CFRPs composites, which exhibited the potential for application in other metal–matrix-bonding composite systems.
This study focused on effective methods of laser engraving treatment (LET), plasma spraying, and resin pre-coating (RPC) to manufacture the reinforced adhesive joints of titanium alloy and carbon fiber-reinforced polymer (TA-CFRP) composites. The combined treatments contributed to the creation of a better adhesive bonding condition and offer a vertical gap between circular protrusions to form epoxy pins and carbon nanotube (CNT)-reinforced epoxy pins. The bonding strength of the TA-CFRP composite was reinforced by 130.6% via treatments with a twice-engraving unit of 0.8 mm, plasma spraying, and RPC. The original debonding failure on the TA surface was changed into the cohesive failure of the epoxy adhesive and delamination-dominated failure of the CFRP panel. Overall, laser engraving has been confirmed as an effective and controllable treatment method to reinforce the bonding strength of the TA-CFRP joint combined with plasma spraying and RPC. It may be considered as an alternative in industry for manufacturing high-performance metal–CFRP composites.
Carbon fiber-reinforced polymer (CFRP) composites have excellent mechanical properties, but their performance is hampered by delamination caused by weak interfacial bonding and resin-rich region (RRR). This research has proposed an interleaving film to improve interlaminar structure and mechanical properties by adding polyacrylonitrile (PAN) fiber into the epoxy interlayer of the CFRP laminates. The PAN fiber/epoxy resin (PANER) interleaving film could be prepared, which was beneficial to hinder crack initiation paths and improve the load transfer. Flexural and compression performance testing results showed optimum performance was obtained when 2 wt.% PAN fiber was added, and an increment of 28.6% was obtained in the flexural strength and 11.7% increment in compressive strength. The damaged energy absorption was improved up to 21.4% and 11.3% for the flexural and compressive properties, respectively. The overall thickness increments in the interlayer with PANER interleaving film were approximately 4–9 μm. X-Ray micro-computed tomography and scanning electron microscopy observations exhibited the potential of PAN fiber in the reduction of RRR, resulting in modes replacement from delamination-dominant failure to crossing-multi-layer failure. In all, PANER interleaving film at the interlayer has been confirmed to be an effective approach to produce a simple reinforcement technology for FRP laminates.
This study designed laser engraving and resin pre-coating (RPC) treatments on an aluminum alloy (AA) surface to construct through-the-thickness “epoxy pins” for improving the bonding strength with carbon fiber reinforced polymer (CFRP). A laser engraving treatment was used to create a pitted structure on the AA surface; higher wettability was acquired and greater vertical spaces were formed to impregnate epoxy resin, resulting in stronger mechanical interlocking. The RPC technique was further used to guide high-viscosity epoxy resin into pits to form the epoxy coatings and to minimize defects between the resin and the substrate. The bonding strength of the specimen treated with both laser engraving with a unit dimension of 0.3 mm and RPC increased up to 227.1% in comparison with that of the base. The failure modes of the hybrid composites changed from the debonding failure of the AA surface to the delamination-dominated failure of the laminated CFRP composites. It was confirmed that laser engraving is a feasible and effective method when combined with RPC for treating AAs to improve the bonding strength of AA-CFRP composites, which provides a reference for preparing high-performance hybrid composites with metals.