The paper considers the results of the application of dry magnetic separation on samples of ferruginous quartzites of the Kostomuksha ore field, represented by refractory ore, free-milling ore, and their mixture. The assessment of the influence of the ore texture on the technological parameters of dry magnetic separation indicates their insignificant changes: the yield of the non-magnetic product varies from 12.4 to 13.5%, and the Fetotal content in the magnetic product increases by 1.11–1.14 times. A decrease of at least 15% in the number of harmful impurities was found: S by 16.2–17.3%, SiO2 by 15.5–21.1%, and Al2O3 by 39.1–48.4%. The authors have performed a comparative assessment of the granularity of the initial ore and the magnetic product with the measurement of energy consumption, as well as an analysis of the magnetite liberation on particle sizes of less than 2 mm. It was found that due to the release of a non-magnetic product in the amount of 12.3–14.5%, represented by non-magnetite or weakly mineralized rock varieties, energy consumption for the crushing process is reduced by at least 5%. The mineral liberation assessment showed that mainly free magnetite is contained in the −0.4 mm fineness class. It was found that in the magnetic separation product of the refractory ore sample, the amount of liberated magnetite in the size class −1 + 0 mm increases by 12.1% compared to the initial ore sample. For the free-milling ore sample, the opposite trend is observed: a decrease in the amount of free magnetite by 30.9% in the magnetic product. Analysis of the magnetite liberation in the mixture indicates deterioration in the results obtained during the separate crushing of refractory and free-milling ore and a decrease in the amount of liberated magnetite in the magnetic product by 60% compared to the initial ore.
On the example of a sample of ferruginous quartzites from the Olenegorskoye deposit, the possibility of preliminary concentration by dry magnetic separation (DMS) has been established. The mineralogical and petrographic studies have shown that, in terms of their textural and structural features and mineral composition, ferruginous quartzites may be divided into two types, differing in the amount of hematite included in their composition, which indicates the possibility of using DMS to generate the following three separation products: magnetite, hematite-magnetite, and rock. DMS with the use of a laboratory drum magnetic separator allowed selecting the upper size limit of 80 mm for lumps entering the separation. At the same time, 24.7 to 26.0 % of all waste and low-mineralized rocks with the mass fraction of Fetot of 4.51 to 6.07 % are transferred to the non-magnetic fraction during the separation of classes of –80+50 and –50+25 mm. For the size class of –25+10 mm, the yield and Fetot values are within the same limits. It has been shown that sulfidecontaining rocks and rocks of increased strength (with the strength coefficient of at least 23) are separated into the non-magnetic fraction. The strength of ferruginous quartzites does not exceed 20. This rock strength ratio confirms improved crushing and grinding efficiency. The possibility of separation of the magnetic fraction with the particle size of –80+25 mm into the following products has been established: the magnetite-hematite product (MF-1 + MF-2) with the mass fractions of Femagn 43.3% and Fehem 14.9 %, and the predominantly hematite product (MF-3 + MF-4) with the mass fractions of Femagn 1.1 % and Fehem 67.9 %.
The article presents the results of the first study stage aimed at analyzing the luminescent properties of the main and minor minerals composing the apatite–nepheline ores and host rocks in the deposits of the Khibiny rock massif (Kola Peninsula, Russia). The main purpose of the work was a search of a stable identification feature providing fast and safe determination of fluorapatite in the mineral mixture of apatite–nepheline ores and solving technological tasks, namely sampling the borehole walls in open pits. The first stage includes studies carried out on pure mono-fractions of four minerals occurring in fluorapatite deposits and possessing obvious luminescent properties: fluorapatite, nepheline, calcite, and sodalite. The authors have revealed luminescence spectra of these minerals and established correlation of their spectral characteristics with the literature data and their consistency. However, the high intensity of sodalite luminescence in a wide band can complicate identification of fluorapatite by the luminescence spectrum in many cases. Therefore, it is reasonable to use the color and intensity of luminescence rather than spectral characteristics.
This article presents developed hardware and software solutions based on the application of machine vision technology. The hardware and software solutions were created in order to generate a database of HSV-color value for the main ore types, host rocks, and minerals to define criteria for the in-process identification of the Khibiny apatite in testing the walls of blasting boreholes. The hardware ensures a multi-parametric assessment of the optical characteristics of samples and minerals located on their surface. The designed software solution allows the user to control the measurement process; systematize a description of the textural and structural features of the sample under study; and process images of the core surface. The resultant database of HSV-color value for the main ores and rocks of the Khibiny massif and their constituent minerals will provide an opportunity to search for criteria for the in-process identification of the Khibiny apatite in a mineral mixture.
The article presents evaluation of preparability of iron ore from Yakovlevo deposit, Kursk Magnetic Anomaly, using magnetic, gravity and X-ray radiometric methods of coarse particle separation. The detailed study involved a material with particle size of \(-100+25\) mm, containing 25–45% Fe\(_\mathrm{total}\) and 3–35% of Fe\(_\mathrm{magn}\) and requiring dressing. It is found that effective separation of the initial feedstock into ore and dirt is ensured by the X-ray radiometric method of separation of coarse particles \(-50+25\) mm in size. At the analytical parameter equal to 2, the increase in the content of Fe\(_\mathrm{total}\) in the ore product reaches 1.18 times at the loss of 5.52%.
This paper presents an engineering evaluation of the possibility of processing the balance reserves and the low-grade apatite ores (LGAO), stored in special dumps, by including lump magnetic separation in the ore preparation technology. The total iron content (Fetotal) in LGAO is more than two times lower than the standard value for the copper concentrator of Kovdorsky GOK. Based on the results of chemical and petrographic analyzes and the development of correlation plots for the magnetic susceptibility and Fetotal and dressability curves for Fetotal and P2O5, respective threshold magnetic susceptibility values were substantiated and three separation products were formed (magnetic product, rock product and middlings). This increased the total iron content in the magnetic product by a factor of 1.9, which now enables its processing using the existing technology for the production of an iron ore concentrate. The total iron losses with the rock product amounted to 6 %. An iron ore concentrate was obtained from the separated magnetic product using the process consisting of a crushing stage, wet magnetic separation stage I to generate the magnetic fraction, its grinding in a ball mill and wet magnetic separation stages II, III and IV to obtain a conditioned magnetite concentrate with the mass fraction of Fetotal of 64.15 % and the recovery of 75.5 % for the magnetic product of lump magnetic separation.