A model based in COMSOL Multiphysics consisting of an electrorefining cell was utilized to simulate copper electrorefining. Concentration and electrolyte density profiles were generated as electrochemical simulation results. Fluid velocity field, particle trajectories, and particle distribution maps were generated to study impurity particle behavior in electrolyte. A three factor designed set of boundary conditions was used to determine the effects of inlet flow rate, temperature, and current density on impurity particle behavior in electrolyte and the associated distribution on the cross section (slice) 100 microns away from the front surface of the cathode during copper electrorefining. The number of impurity particles on the cross section was counted for each set of boundary conditions. The model data for impurity particle distribution was compared with measured impurity particle contamination at the cathode surface, and the results show a very good correlation, which suggests the model is reasonable. The model results show the three factors have significant effects on the number of impurity particles on the cross section. The impurity particle counts at the corner positions of the slice are much higher than those at the center position of the slice. Possible explanations for the simulation results are proposed.
Copper electrorefining tests were conducted in a pilot scale cell made of transparent cell walls, allowing direct observation and microscopic video recording of the electrolyte flow. Fluid flow velocities in the gaps between adjacent anodes and cathodes were measured by analyzing the recorded video using a video analysis and modeling software. Modeling and simulation of copper electrorefining in this cell were performed using COMSOL Multiphysics, a finite element method simulation software. The flow velocity field results from modeling agree reasonably well with the measured electrolyte velocities. The transport of slime particle in electrolyte flow was also simulated and the appearance frequencies of slime particles in the domain within 200 microns from cathode surface at different positions of cathodes were compared with impurity levels in the copper cathodes harvested from experimental tests. The results show good correlation especially with the total concentration of major impurities. Thus the cathodic contamination can be predicted by the slime particle appearance frequency in front of the cathode.
19 November 2015 in Journal of the Electrochemical Society
Four series of copper electrorefining tests were performed using four different types of anodes, which have different inclusion types. Test results show that the high impurity anodes and the scrap cycle anodes have more inclusions associated with the Pb-Bi-S compounds that show evidence of sintering at 50°C, whereas the low impurity anodes and the strip cycle anodes have more inclusions related with the Pb-Bi-S-As compounds that demonstrate evidence of sintering above 65°C. Inclusion (slime) particles sinter and adhere to the anode surface, which happens at lower temperatures for the high impurity anodes and the scrap cycle anodes. Correspondingly, there are different slime distributions for each type of anode. The anode slimes layers in front of anode surfaces for different types of anodes were observed and analyzed by SEM/EDS. Results show significant effects of particle sintering near anode surfaces, which was also demonstrated by slime size distributions at different cell temperatures. Experimental results demonstrate that slime particle sintering and coalescence can improve anode slime adhesion and reduce the amount of suspended slimes, which are a major source of copper cathode contamination. Arsenic content in copper anode and cell temperature are major factors affecting slime sintering and coalescence.