Blue sapphire has long been treated with heat to modify its blue color and attain greater value. However, the process of modifying the blue color in sapphire remains not well understood. The color-changing mechanism has traditionally been explained using the Intervalence Charge Transfer (IVCT) (Fe2+-Ti4+ and/or Fe2+-Fe3+) theory, wherein the blue color can be diminished by heat treatment in an oxidizing environment which alters Fe2+ (FeO) to Fe3+ (Fe2O3) and decreases the occurrence of the IVCT process. However, recently, the band gap theory has been proposed, suggesting that iron (Fe) in sapphire is always in the Fe3+ state, the blue color is caused by Fe3+-Ti4+ pair and the heat treatment does not affect Fe oxidation state. Therefore, in this study, eight magmatic sapphires from four localities were investigated for changes in blue color via color analysis, changes in spectra using XANES, and changes in chemical composition using PIXE both before and after heat treatment. The color analysis reveals a slight reduction in saturation (fading of blue) and a noticeable lightening after heat treatment, which corresponds with the high content of solid inclusions or trapiche samples. XANES data analysis using the LCF technique indicated insignificant changes in Fe oxidation state from 2+ to 3+ after heat treatment across all samples. However, when comparing the XANES data with color parameter L*a*b*, it is noted that the percentage of Fe oxidation state changes does not show a positive relationship with changes in blue based on color parameter b* (blue–yellow); rather, it shows a positive relationship with parameter L* (lightness). Microscopic observations also reveal the dissolution of clouds or minute particles around planes of ilmenite needles. It could be suggested that the changes in Fe oxidation state may not be directly related to changes in blue color but could be linked to the partial dissolution of Fe-bearing inclusions.
Low-temperature heat treatment in magmatic sapphires can be difficult to detect because conventional indicators, including hydroxyl-related absorptions and short-wave ultraviolet fluorescence, are often weak, absent, or inconclusive in Fe-rich material. This study evaluates Fourier transform infrared (FTIR) reflectance spectroscopy as a method for detecting low-temperature heat treatment in Vietnamese magmatic sapphires. A total of 38 natural sapphires from basalt-related deposits in southern Vietnam, comprising 23 samples from Dak Lak and 15 samples from Phan Thiet, were analyzed before and after heating at 1100 °C for 3 h under oxidizing conditions. Particular attention was given to spectral modifications within the fingerprint region (1000–500 cm−1), which is dominated by lattice-vibrational modes of α-Al2O3. Following heat treatment, all samples exhibited a systematic shift in the dominant reflectance trough-center position from 646.4 ± 2.0 cm−1 to 630.2 ± 0.8 cm−1 together with a substantial increase in trough depth from 0.052 ± 0.025 to 0.705 ± 0.118%R (p < 0.0001). The spectral feature also became narrower and more sharply defined after heating, consistent with modification of the local vibrational environment within the corundum lattice. In contrast, hydroxyl-related absorptions in the 3100–3700 cm−1 region were weak, variably developed, or absent and showed no reproducible treatment-related behavior. Complete separation between untreated and heat-treated samples was achieved when trough-center position and trough depth were evaluated jointly. These results demonstrate that FTIR fingerprint-region parameters derived from intrinsic α-Al2O3 lattice vibrations provide robust indicators of low-temperature heat treatment in Vietnamese magmatic sapphires and may serve as complementary criteria when conventional OH-based indicators are inconclusive.