PHBV films incorporating 3, 6 and 9% ferulic acid (FA) or p-coumaric acid (PCA) were obtained by melt blending and compression moulding. The films’ microstructures and thermal behaviours were analysed as well as their mechanical, optical and barrier properties. The overall and specific migration of the materials in different food simulants was also characterised. FA was homogeneously mixed with the polymer, whereas PCA was mainly dispersed as fine particles in the PHBV matrices due to its higher melting point. These structural features promoted differences in the physical properties of the films depending on the compound concentration. As the concentration of both compounds rose, the barrier capacity of the films to oxygen, and to a lesser extent water vapour, was enhanced. While FA promoted the extensibility of the films, 9% PCA enhanced their brittleness. Both compounds affected the crystallisation pattern of the polymer, promoting smaller crystalline formations and a slight decrease in crystallinity. Although the overall migration of every film formulation was lower than the overall migration limit (OML), the release of active compounds was dependent on the food simulant; almost total release was noted in ethanol containing simulants but was more limited in aqueous systems. Therefore, these films could be used as food contact materials, contributing to extending the food’s shelf life.
Poly(3-hydroxybutyrate-co-3-hydroxyvalerate) (PHBV) is a biodegradable biopolymer from the PHAs family that has potential to replace conventional plastics and reduce plastic pollution. However, PHBV has thermo-sealability issues, making it challenging to use for bags. Blending it with polycaprolactone (PCL) could address this but may alter the barrier properties of the films, affecting their effectiveness as food packaging material. This study examined the properties and heat-sealing capacity of PHBV/PCL blend films (ratios: 60/40, 50/50, and 40/60), obtained by melt blending and compression moulding. Both polymers are immiscible and were in separated phases; the continuous phase was PHBV in the 60/40 blend and PCL in the 40/60 blend, while the 50/50 sample exhibited interpenetrating bicontinuous phases of both polymers. The permeability to water vapour, oxygen, and D-limonene increased as the PCL content rose, especially when it formed the continuous phase in the matrix. The elastic modulus and resistance to break decreased, while extensibility increased, more markedly when PCL was the continuous phase. However, the continuity of PCL phase provided the films with better thermal adhesion and seal strength. The 50/50 blend showed the best balance between heat sealability and barrier properties, making it the most suitable for food packaging in sealed bags.
The biodegradation of polymer films is affected both by their composition and structure and by the environmental conditions. Composting behaviour of poly(hydroxybutyrate-co-hydroxyvalerate) (PHBV) films was studied at lab-scale, according to ISO 20200:2023, as affected by its blend (1:1) with polycaprolactone (PCL), and the presence (6 % wt.) of active compounds (Ferulic acid: FA, and rice straw extract: RSE). The film disintegration (mass loss) was monitored over the composting time, by microstructural analysis, FTIR spectroscopy, and thermal analyses. All films disintegrated completely at the end of the test (84 days), but the disintegration rate was affected by the formulation. PHBV and blends films containing RSE exhibited the fastest disintegration whereas blend films without actives were the slowest. In every case, the surface erosion provoked by the biofilm action was the main mechanism responsible for the film thinning, but bulk hydrolysis also occurred to a different extent. RSE, with high content of carbohydrates, promoted the film porosity and bulk hydrolysis of both PHBV and its blend with PCL where the crystallinity of PCL was promoted. FA also accelerated the hydrolysis of the PHBV amorphous phase as well as the crystalline phases of PCL, as deduced from DSC analysis. Therefore, degradation rate was affected by overlapping of the different mechanism, depending on the film composition and structure. Promoting the water diffusion through the film favoured the hydrolytic processes and the enzymatic action of the biofilm microorganisms, whose population and activity could also be affected by film components.