In this paper, the electrical behavior of tungsten carbide (WC) Schottky barrier on 4H-SiC was investigated. First, a statistical current-voltage (I–V) analysis in forward bias, performed on a set of equivalent diodes, showed a symmetric Gaussian-like distribution of the barrier heights after annealing at 700 °C, where a low Schottky barrier height (Φ B = 1.05 eV) and an ideality factor n = 1.06 were measured. The low value of the barrier height makes such a WC contact an interesting candidate to reduce the conduction losses in 4H-SiC Schottky diodes. A deeper characterization has been carried out, by monitoring the temperature dependence of the I–V characteristics and the behavior of the relevant parameters Φ B and n. The increase of the barrier height and decrease of the ideality factor with increasing temperature indicated a lateral inhomogeneity of the WC/4H-SiC Schottky contact, which was described by invoking Tung’s model. Interestingly, the temperature dependence of the leakage current under reverse bias could be described by considering in the thermionic field emission model the temperature dependent barrier height related to the inhomogeneity. These results can be useful to predict the behavior of WC/4H-SiC Schottky diodes under operative conditions.
10 December 2021 in Semiconductor Science and Technology
In this paper, we investigate the electrical evolution of tungsten (W) and tungsten carbide (WC) Schottky contacts on 4H-SiC subjected to thermal treatments at different annealing temperatures from 475 °C to 700 °C. For each annealing temperature, the uniformity of the Schottky barrier height (ΦB) and ideality factor (n) was monitored by current–voltage (I–V) measurements in forward bias, performed over sets of equivalent diodes. Good values of n (below 1.05) were found for both contacts up to thermal annealing at 700 °C. On the other hand, the barrier of the two contacts behaves differently. For the W/4H-SiC diode, the ΦB increases with the annealing temperature (from 1.14 eV at 475 °C to 1.25 eV at 700 °C), whereas the Schottky barrier in WC/4H-SiC features a slight reduction already with thermal annealing at 475 °C, remaining almost constant at around 1.06 eV up to annealing at 700 °C. A deeper characterization was performed on the 700 °C-annealed contacts by studying the temperature-dependence of the Schottky parameters by current–voltage–temperature (I–V–T) characterization. The ΦB and n behaviour with temperature indicates the presence of a nanoscale lateral inhomogeneity for both Schottky contacts, which can be described by Tung’s model. Finally, the temperature-dependence of the reverse characteristics could be described by the thermionic field emission model, accounting for the temperature dependent barrier height determined from forward characterization.
New generations of SiC power devices require to be fabricated on very thin substrates, in order to significantly reduce the series resistance of the device. The role of thinning process on the formation of backside ohmic contact has been investigated in this work. Three different mechanical grinding processes have been adopted, resulting in different amounts of defectivity and surface roughness values. An excimer UV laser has been used to form a Ni-silicide based ohmic contact on the backside of the wafers. The reacted layer has been studied by means of Atomic Force Microscopy (AFM), Transmission Electron Microscopy (TEM) and X-Ray Diffraction (XRD) analyses, as a function of grinding process parameters and laser annealing conditions. The ohmic contact has been evaluated by measuring the Sheet Resistance (Rs) of silicided layers and the Vf at nominal current of Schottky Barrier Diode (SBD) devices, fabricated on 150 mm-diameter 4H-SiC wafers. A strong relationship has been found between the crystal damage, induced by thinning process, and the structural, morphological and electrical properties of silicided ohmic contact, formed by UV laser annealing, revealing that the silicide reaction is moved forward, at fixed annealing conditions, by the increasing of crystal defectivity and surface roughness of SiC.
In this paper, we investigated the effects of the processing parameters, such as deposition methods, annealing temperature, and metal thickness, on the electrical characteristics of Ti/4H-SiC contacts. A reduction of the Schottky barrier height from 1.19 to 1.00 eV following an increase of the annealing temperature (475–700 °C) was observed for a reference contact with an 80 nm-thick Ti layer. The current transport mechanisms can be described according to the thermionic emission (TE) and thermionic field emission (TFE) models under forward and reverse biases, respectively. The comparison with an e-beam evaporated Ti(80 nm)/4H-SiC contact did not show significant differences for the forward characteristics, while an increase of the leakage current was observed under high reverse voltage (>500 V). Finally, a thickness variation from 10 to 80 nm induced a reduction of the Schottky barrier height, due to the reaction occurring at the interface with a Ti-Al region extended up to the 4H-SiC surface. In addition to a deeper understanding of the Schottky barrier properties, this work is useful for the development of Schottky barrier diodes with tailored characteristics.