Coiled tubing (CT) is used as a velocity string to transport high-velocity gas in drainage gas recovery technology. Sand particles flowing at high speed can cause serious erosion of the pipe wall. Long-term erosion wear leads to the degradation of the string strength and can even cause local perforation. In order to study the erosion wear problem of CT, a gas–solid erosion experimental device was established for a full-size pipe with different radii of curvature. A 3D laser confocal technique was used to examine and characterize the microscopic erosion morphology of the inner wall of the CT. The CFD erosion model was selected based on the erosion test data of the inner wall of the CT, and the erosion results of the Finnie model show minimal error and good agreement compared with other models. The average value of the error of the maximum erosion rate at different radii of curvature is 8.3%. The effect of the radius of curvature, gas velocity and solid particle size on the maximum erosion rate of the inner wall of the CT was analyzed based on the Finnie model. The results reveal that erosion wear occurs on the inner wall of the CT’s outer bend. As the radius of curvature is reduced, the maximum erosion rate and area increase, and the position of the maximum erosion rate gradually shifts toward the inlet. The maximum erosion rate is positively correlated with the gas flow rate. However, as the particle size increases, the maximum erosion rate shows a trend of first increasing, then decreasing and finally stabilizing, with a critical particle size of 200 μm. This study can provide theoretical guidance and methods for improving the service life of CT. The erosion rate of the tubing in old wells can be reduced by controlling production and employing appropriate sand control methods, while the erosion rate of tubing in new wells can be reduced by adjusting the wellbore trajectory.
Corrosion failure of oil well tubing in the ocean can lead to significant economic losses. Surface treatment is often used to enhance the corrosion resistance of tubing, while corrosion acceleration will occur in a certain environment. This work combined onset failure analysis and corrosion simulation measurements to understand the failure procedure and corrosion mechanism of nickel plating materials in calcium chloride water-type weak corrosion environment. The microscopic analysis results of the failed part show CO2 corrosion products co-deposit with SRB bacterial sulfide products and Ca compounds. The damage of nickel plating is accompanied by S-containing products, which was confirmed by simulated immersion experiments at 50 °C, 0.28 MPa CO2 partial pressure, and a speed of 3 m/s. The aggressive solution penetrates through the micro-damage pores, followed by the degradation of the Ni plating layer into NiS, leading to the localized loss of protection and triggering under-deposit corrosion. Concurrently, the SRB’s anaerobic environment generates CO2 corrosion byproducts and SRB-derived FeS.
In 2023, two wells in the NB 35-2 field had not yet begun to inject heat, and the temperatures in the 0-400m depth region of the formation were significantly higher than the values of the normal ground temperature gradient. Numerical simulation studies are carried out in order to investigate the reasons for the shallow formation temperature anomalies and to clarify the impact of heat injection wells on the surrounding area. Finite element numerical simulations were analyzed based on the thermal parameters of nitrogen, casing, cement ring and formation according to the actual well distribution. Numerical simulations of formation temperature changes in NB 35-2 due to production, steam stimulation were carried out. The simulation results show that: (1) the injection of nitrogen during the thermal extraction operation has a good thermal insulation effect, which can seal most of the heat in the tubing and casing annulus. (2) High fluid temperature in the two production wells is the primary cause of high shallow formation temperatures in NB 35-2. (3) In the extreme case, even if the insulated tubing is not working, there is a 3-5 day response time to treat the steam throughput well accordingly before it affects neighboring wells.