This paper presents the results of fire test of an I-beam protected by a combined magnesite plate-magnesite mixture heat-insulating material. It was shown that a composite with an average thickness of 37 mm maintained an average temperature of 380 °C on the metal surface after 150 minutes of fire exposure, not exceeding the critical value of 500 °C. From 60 to 100 minutes of fire testing (furnace temperature of 980-1025 °C), the temperature of the metal did not exceed 100 °C. This was achieved both due to the high thermal insulation properties of the magnesite mixture, and due to gas and vapor release from the hydration products of magnesia cement. The developed fire-retardant material provides the first group of fire-retardant efficiency (150 minutes) and, after the fire test, is characterized by density of 352.4 kg/m3 and compressive strength of 0.85 MPa, which is three times lower than the original.
18 June 2021 in Eastern-European Journal of Enterprise Technologies
This paper reports the principles of design and the examined protective properties of liquid materials for shielding the electric, magnetic, and electromagnetic fields over a wide frequency range. The materials were made on the basis of iron ore concentrate and a pigment additive, with water-dispersed and geopolymer paints used as a matrix. The tests of protective properties for the electrical and magnetic components of the electromagnetic field of industrial frequency showed that the electric field shielding coefficients at a concentration of the screening substance of 15−60 % (by weight) equaled 1.1−8.6; magnetic field – 1.2−5.3. The shielding coefficients of the material based on a water-dispersed paint are lower than those of a geopolymer one, which can be explained by the oxidation of an iron-containing component and a decrease in electrical conductivity. The shielding coefficients of the electromagnetic field with a frequency of 2.45 GHz are 1.2−7.9. The highest coefficients are inherent in the material with filler made of iron ore concentrate and titanium-containing pigment powder in a ratio of 1:1. To design materials with the required (predictable) protective properties, the relative magnetic, dielectric permeability of materials was calculated. It is shown that the obtained data are acceptably the same as the results from direct measurements of magnetic and dielectric permeability and could be used to calculate the wave resistance of the material and the predicted reflection coefficient of electromagnetic waves. Thus, there is reason to assert the need to build a database on the frequency dependence of effective magnetic and dielectric permeability in order to automate the design processes of composite materials with predefined protective properties.
The purpose of the work was to study physico-mechanical properties of glued connections of wood rods, toothed lamellae after splicing and corner spike clamping of window frames which were obtained in the production conditions. The alkaline aluminosilicate binder-based adhesive (glue) of the composition 0.8Na2O·Al2O3·4.5SiO2·20H2O modified using organo-mineral additives was used in testing. After solidification of the adhesive, the samples were cut to determine the strength of frame corner joints in bending, glued timber connections for splitting along the grains, toothed glued connections in bending and water resistance of the glued connections of timber elements. The results of these tests showed high values of strength characteristics in case of the proposed modified alkaline aluminosilicate binder-based adhesive (glue), which were by 1.5 times higher than those in case of the WoodMax (D2) taken as a reference glue, and in water resistance complied with Class D2/D3 as per PN-EN 204.
8 May 2019 in Eastern-European Journal of Enterprise Technologies
The paper presents data on the use of the alkaline aluminosilicate binder-based adhesive of the system Na2O•Al2O3•(4-6)SiO2•(17-20)H2O for gluing and fire protection of structural timber elements. The results of the study of thermoresistant phases in the reaction products of the alkaline aluminosilicates are reported and discussed. The results allowed to show that at SiO2/Al2O3 between 5 and 6 the zeolite-like phases of heulandite types, which, under action of temperatures, are able to form a porous aluminosilicate artificial stone with low thermal conductivity (λ=0.09 Wt/m•К, DSTU B V.2.7-105-2000 (GOST 7076-99)) are formed in the reaction products. The use of the developed aluminosilicate adhesives allow for to classify the structural timber elements as hardly burnable and hardly flammable materials (GOST 12.1.044-1989, EN 13823 + A1: 2014-12, ASTM E119-07). They have the following characteristics: water resistance D3 (EN 204:2001), resistance in splitting up 7.8 MPa (GOST 16483.5-1973), adhesion in normal pull-off test up to 2.6 MPa (GOST 32299-2013 (ISO 4624:2002)).
3 December 2019 in Eastern-European Journal of Enterprise Technologies