Effect of rare earth element La on non-oriented electrical steel produced by thin slab casting and rolling process is investigated by using transmission electron microscope, scanning electron microscope and X-ray diffraction. The results show that, (1) The columnar crystals are refined obviously with the addition of rare earth element La, the primary dendrite arm spacing is reduced from 2.42 mm to 1.76 mm, and the secondary dendrite arm spacing is reduced from 0.35 mm to 0.28 mm. (2) The banded structure of the hot rolled plate in center is significantly improved after adding rare earth, the thickness of the banded structure is reduced from 0.75 mm to 0.24 mm. (3) With the addition of rare earth element La, the precipitation morphology of AlN transforms from lump to spherical, the density and amount of inclusions are greatly reduced. (4) The average grain size of finished product is increased with the addition of rare earth element La, meanwhile, the unfavorable texture of (111) decreases and the favorable texture of (100) and (110) increases. With the addition of rare earth, the average core loss is decreased by 0.4 W/kg, and the average magnetic induction intensity is increased by 0.011T.
26 August 2019 in Metallurgical Research & Technology
The grain-oriented silicon steel was produced by medium temperature reheating and two-stage cold rolling process, and the microstructure and texture of all metallurgical processes were studied. The results shown that the microstructure of the hot rolled strip was inhomogeneous in thickness direction, the surface layer was the recrystallized microstructures with average grain size of 42.29 µm, the center layer was fiber structure, and the Goss texture appeared at surface. The primary recrystallized microstructure with average grain size of 16 µm was obtained after decarburization annealing, which characterized by a strong γ-fiber texture and a weak Goss texture. The average size of inhibitors in hot rolled strip and decarburization annealed sheet were 9.078 and 21.691 nm respectively, they were mainly compound of nitride and sulfide with spherical or lump shapes. The coarse Goss grains with average size 17.57 mm were got after secondary recrystallization, and the magnetic induction B8 and iron loss P1.7/50 were 1.885 T and 1.10 W/Kg, respectively.
8 September 2020 in Metallurgical Research & Technology
The medium temperature reheating and two-stage cold rolling process were adopted to produce industrialized Grain-oriented silicon steel. Results showed there were three sections (surface layer, transition layer and central layer) along the thickness direction on hot rolled sheets. Surface layer was occupied by complete recrystallization grains with average grain size 42.81 mu m, while the central layer mainly consisted of fibrous microstructure. The Goss texture appeared only on surface layer with content 3.44%similar to 3.65%. After the first cold rolling with 72% reduction and decarburization annealing, the primary recrystallization occurred and average grains size reached 19.0 mu m, simultaneously accompanied with texture rotated to lambda, gamma fiber texture and Goss texture dropped to 2.89%. Adopting the second cold rolling with 58% reduction, the cold rolled sheet consisted of deformed fiber microstructure and the texture maintained gamma fiber texture with a peak at {111} . The precipitates in hot rolled sheets comprised Cu2S and few AlN, and the average particle size was similar to 14nm. The inhibitors in the decarburization annealing sheet were mainly AlN, Cu2S, MnS and their composite precipitation, which were spherical or massive with the average particle size similar to 21nm. The single Goss oriented grains with average grain size 9.41mm were obtained after high temperature annealing, and the intensity reached 873.30. The final magnetic properties were: B-8=1.865T and P-1.7/50=1.124W/kg, which met the requirement of 27Q120.