The influence of nominal Pt underlayer thickness on in-plane magnetization reversal was investigated in Pt(t)/Co(5 Å)/Pt(5 Å)/CoO(100 Å)/Pt(10 Å) heterostructures deposited on polyethylene terephthalate (PET), with t = 5, 10, 15, and 20 Å. Room-temperature angle-dependent longitudinal magneto-optical Kerr effect (MOKE) measurements revealed distinct responses across the series rather than a simple monotonic thickness trend. Pt5 showed weak angular coercivity variations, Pt10 yielded no reliably resolvable MOKE hysteresis loop, Pt15 exhibited measurable hysteresis with substantial scatter in angular coercivity, and Pt20 displayed pronounced angular modulation. Empirical harmonic analysis favored a fourfold contribution for Pt20 within a selected background model, but did not establish fourfold magnetocrystalline anisotropy. Following a single field-cooling procedure under an in-plane field of +150 mT, superconducting quantum interference device (SQUID) measurements of Pt20 revealed a positive loop-center displacement that reached approximately 3.76 mT at 120 K before decreasing to approximately 1.46 mT at 100 K. The additional low-temperature displacement is compatible with a possible exchange-bias contribution, although its intrinsic magnitude and microscopic origin remain unresolved. These findings demonstrate Pt-underlayer-sensitive magnetization reversal and a distinct temperature-dependent loop displacement in Pt20.