A microspherical hybrid fibroin-silica adsorbent (HFSA) was prepared and evaluated as a multifunctional stationary phase for the thin-layer chromatographic analysis of structurally diverse dyes. The material was synthesized by adding silk fibroin during the hydrolytic polycondensation of tetraethoxysilane (TEOS) and characterized using SEM-EDS, FTIR spectroscopy, XRD, and nitrogen adsorption-desorption analysis. HFSA exhibited a predominantly amorphous, microspherical, and porous structure, with a specific surface area of 318 m2/g and a total pore volume of 1.03 cm3/g. The chromatographic behavior of methyl orange, Sudan I, Sudan IV, and Rhodamine 6G was investigated by TLC using MPh1 [n-hexane:isopropanol (1:1, v/v)] and MPh2 [n-hexane:isopropanol:water:glacial acetic acid (1:1:0.5:0.1, v/v/v/v)]. Under MPh1, all four dyes exhibited greater apparent retention on HFSA than on microspherical silica gel (MSS), with the largest observed difference for Sudan IV. Introducing water and acetic acid markedly changed the migration order: Sudan IV and Sudan I became highly mobile, whereas methyl orange and Rhodamine 6G remained more strongly retained. A dimensionless retention transport reconstruction reproduced the experimental band-centroid positions and visualized condition-dependent migration without independently predicting experimental band broadening or resolution. Hydrogen bonding, hydrophobic association, van der Waals forces, π–π interactions, and possible electrostatic effects are proposed as contributions to retention; their individual roles were not experimentally distinguished. These findings demonstrate that HFSA provides a chemically diverse stationary phase that exhibits different retention behavior for the four investigated dyes under the two tested mobile-phase conditions.
29 May 2026 in Himia, Fizika ta Tehnologia Poverhni
The main aim of this work is to synthesize microspherical fibroin/silica adsorbent through a one-step in situ synthesis that integrates silk fibroin into the hydrolytic polycondensation of tetraethoxysilane (TEOS). The kinetics of the sol-gel process is studied at varying ratios of the initial reagents - fibroin, TEOS and ammonium hydroxide in a 4% formic acid solution under different temperatures and stirring rates. It was demonstrated that the sol-gel transition in all cases occurs within a few minutes. The highest yield of the target product was observed at a fibroin:TEOS ratio of 0.03:1 and the addition of 2.3 ml of 25 % ammonium hydroxide solution. The obtained samples were analyzed using scanning electron microscopy with EDS, nitrogen porosimetry, IR spectroscopy, diffractometry and thermogravimetry. The morphologically obtained fibroin/silica adsorbent consists of microspherical particles measuring 10 ?m in size, with a pore size distribution of 10–30 nm and a specific surface area of 318 m2·g-1. The IR study of the obtained nanohybrid fibroin/silica adsorbent reveals absorption bands at 3410 cm–1 characteristics of ?Si-OH groups and at 1063 cm–1 related to vibrations of the siloxane group ?Si-O-Si? in the silica structure. The characteristic absorption bands of Amide I at 1638 cm–1 and Amide II at 1512 cm–1 confirm the presence of fibroin. The interactions between fibroin macromolecules and the formed silica structure are evidenced by a reduction in crystallinity of the fibroin within the obtained samples. The nitrogen adsorption and desorption isotherm reveals the presence of a hysteresis loop, indicating that the obtained nanohybrid fibroin/silica adsorbent possesses the mesoporous structure. According to the IR spectral, X-ray structural and thermal characteristics, the obtained product comprises silica and fibroin phases and differs from its constituent components, which confirm its nature as a hybrid nanocomposite material. Additionally, its potential application for separating nitroaniline isomers using high-performance thin-layer chromatography has been demonstrated.