In this study, single and duplex aging treatment was applied to the metastable beta titanium alloy of titanium-15 vanadium-3 aluminum-3 chromium-3 tin with cryogenic treatment. The single-step aging treatment was applied for 20 h at 450°C and 10 h at 550°C. The cryogenic treatment was carried out at −196°C for 24 h, followed by single-step or duplex aging treatment. The results obtained show that the cryogenic treatment causes the formation of martensitic alpha phases. Following the cryogenic treatment, martensitic alpha phases were observed in the sample, which was subjected to aging treatment at 450°C for 20 h, whereas these phases disappeared completely in the sample treated at 550°C for 10 h. Preaging treatment applied after cryogenic treatment prevented the formation of precipitate-free zones by providing a finer and uniform distribution of α phases. Cryogenic treatment followed by preaging treatment at 250°C for 24 h led to the formation of dense metastable prephases. This resulted in a 10% increase in tensile strength, 4% elongation, and 5% hardness compared to preaging at 300°C for 10 h after cryogenic treatment. The optimum mechanical properties in single-step sample groups were obtained in samples aged 20 h at 450°C. In duplex-aged samples, optimum mechanical properties were obtained in cryogenic treatment followed by 250°C/10 h + 450°C/20 h duplex aging treatment.
Ti-6Al-4V α/β titanium alloy is used in biomedical applications to produce artificial joints due to its excellent osseointegration property, high corrosion resistance, low density, and low Elasticity modulus compatible with bone structure. Considering the usage area, Ti-6Al-4V alloy is expected to have high tensile properties and high wear resistance. In this study, aging treatment and a combination of aging and cryogenic treatment were applied to the alloy to obtain high tensile properties and wear resistance. Cryogenic treatment was conducted at deep (-196°C) and shallow (-140°C) cryogenic treatment temperatures. Also, aging treatment was conducted to the alloy with/without cryogenic treatment as a single-step or duplex. The effect of the heat treatment types on the alloy's mechanical and microstructural properties was determined by tensile test, hardness test, wear test, XRD phase analysis, and microstructural investigations. With the application of the duplex aging treatment amount of the β phases decreased, a good balance between tensile strength and the elongation was obtained, and the wear resistance of the alloy increased compared to the single-step aging. In addition, the decrease of the cryogenic treatment temperature slowed down the phase transformation kinetics and caused a decrease in precipitation of α phases at both single-step and duplex aged samples. Superior wear resistance was obtained with the reduction of β phases in the microstructure of the samples that were duplex aged after cryogenic treatment.
1 December 2022 in Physics of Metals and Metallography
Metastable β titanium alloys were used in the aviation field in the first years of their discovery because of their high strength versus low density, providing fuel savings. However, studies conducted in recent years show that the usage areas of metastable alloys will increase owing to their unique properties, such as high heat treatment efficiency. In this study, corrosion resistance of Ti–15V–3Al–3Sn–3Cr alloy was investigated by applying single-step, duplex aging, and cryogenic treatment to the alloy separately or consecutively. The alloy was heated with an ultra-low heating rate of 0.2°C/min to aging treatment temperature to allow the formation of metastable phases. The cryogenic treatment was applied at –196°C for 24 hours, the single-step aging was conducted at 500°C for 6 hours, and the duplex aging treatments were applied for 24 hours at 250°C followed by 6 hours at 500°C. The corrosion behavior of samples treated at different temperatures was also investigated by Tafel extrapolation and linear polarization methods in 0.9% NaCl solutions at 37°C and 3.5% NaCl solutions at 25°C. The thinnest α phases (width and length 40 ± 7 nm by 170 ± 15 nm, respectively) and the highest microhardness (as 446 HV) were measured in the cryo treated plus duplex aged sample. While the corrosion resistance of the solution-treated Ti–15V–3Al–3Sn–3Cr alloy was highest in both environments, the corrosion resistance decreased with the applied heat treatments.