We have studied the microstructure and optical properties of free-standing porous Si thin films fabricated by electrochemical anodization. Raman-spectroscopy and transmission-electron-microscopy examinations show that Si crystallite spheres with diameters of several nanometers are dispersed in the amorphous phase. The blueshift of the optical-absorption spectrum is observed for decreasing average diameter of the Si crystallites. However, there is no clear size dependence of the peak energy of the broad photoluminescence (PL) spectrum. Spectroscopic analysis strongly suggests that the photogeneration of carriers occurs in the c-Si core, whose band gap is modified by the quantum-confinement effect, while the strong PL comes from the near-surface region of small crystallites.
Porous silicon carbide has been fabricated using single crystal 6H‐SiC that has a wider indirect band gap than silicon crystal. Intense blue‐green luminescence has been observed at room temperature. The peak wavelength is around 460 nm, below the band gap of crystalline SiC. The luminescence intensity is about 100 times stronger than that of crystalline 6H‐SiC. These results not only clarify the origin of luminescence in porous Si but also point to the possibility of the use of this new material for an intense blue‐green luminescent source.
Photoluminescence (PL) and time-resolved PL spectra of zinc oxide (ZnO) films were investigated as a function of the grain size of the microcrystals. Correlation was found between the grain size and the optical properties—in the bound exciton states, both the PL intensity and PL decay time increased with increasing the grain size. This correlation can be well explained by the existence of nonradiative-surface and/or -interface states in the grain boundaries of ZnO microcrystals.
1 April 2005 in Japanese Journal of Applied Physics
We have investigated the defect structure in bismuth titanate (Bi4Ti3O12) through high-temperature neutron powder diffraction analysis and ab-initio electronic structure calculations. It is shown that the vacancies of Bi and oxide ions are created preferentially in the perovskite layers rather than in the Bi2O2 layers. Measurements of the leakage-current properties of the single crystals demonstrate that electron holes arising from the incorporation of oxygen at the vacancies of oxide ions act as detrimental carriers for electrical conduction at room temperature. A crystal growth under high oxygen pressure is proposed to be advantageous for suppressing the vacancy formation and for attaining a large remanent polarization as well as a high insulating property of the Bi4Ti3O12 system.
We have studied the origin of the visible photoluminescence (PL) from oxidized porous Si fabricated by rapid-thermal-oxidization processes. At low oxidation temperature (), the PL spectrum with a peak near 750 nm is observed, and silicon oxyhydrides and silicon oxides are formed at the surface of nanocrystallites. At high above 800 °C, strong blue PL is observed around 400 nm and the surface of crystallites is covered by . The electronic state of porous Si is very sensitive to the surface structure of crystallites. Spectroscopic data indicate that the red PL originates from the near-surface region in the crystallite, while the blue PL originates from the core region in the crystallite.
We have studied and compared the optical properties of both porous Si and the chemically synthesized planar and cubic Si skeleton clusters. Broad photoluminescence with large Stokes shifts were observed at the visible region in both samples. Spectroscopic analysis suggests that the surface of porous Si is similar to a condensation of Si clusters. Small Si clusters play a key role in the strong room-temperature photoluminescence in porous Si.