1 June 1996 in The Journal of Arthroplasty
Damage and rapid wear of the ultrahigh-molecular-weight polyethylene bearings of knee components continue to be major sources of failure of knee prostheses. Despite considerable research into the roles of design, polyethylene thickness and quality, and component alignment, the source of the rapid wear failures has remained a mystery. This study documents elevated oxidation resulting from the use of gamma sterilization in air, the most common sterilization technique used by the orthopaedic implant industry. This oxidation reduces static strength and elongation properties and significantly decreases the resistance of polyethylene bearings to fatigue, a frequent source of early damage of many of these devices.
1 September 2003 in Clinical Orthopaedics and Related Research
Cross-linked polyethylenes are being marketed by orthopaedic manufacturers to address the problem of osteolysis caused by polyethylene particulate wear debris. Wear testing of these cross-linked polyethylenes in hip simulators has shown dramatic reduction in wear rate compared with standard ultrahigh molecular weight polyethylene, either gamma irradiated in air or nitrogen - or ethylene oxide-sterilized. However, this reduction in wear rate is not without cost. The cross-linking processes can result in materials with lower mechanical properties than standard ultrahigh molecular weight polyethylene. To evaluate the effect of the various cross-linking processes on physical and mechanical properties of ultrahigh molecular weight polyethylene, commercially available cross-linked polyethylenes from six orthopaedic manufacturers were tested. This study was the culmination of collaboration with these manufacturers, who provided cross-linked polyethylene for this study, wear characteristics of the material they provided, and review of the physical and mechanical properties measure for their polyethylene. Cross-linked materials were evaluated as received and after an accelerated aging protocol. Free radical identity and concentration, oxidation, crystallinity, melt temperature, ultimate tensile strength, elongation at break, tensile stress at yield, and toughness are reported for each material. By comparing these physical and mechanical properties, surgeons can evaluate the trade-off that results from developing materials with substantially lower wear rates.
1 October 2007 in Journal of Bone and Joint Surgery
Background: Studies have suggested that cross-linked polyethylene bearings reduce wear rates from 40% to 100% compared with conventional polyethylene. However, the reduced mechanical properties of highly cross-linked polyethylene have the potential to be a limiting factor in device performance. We reviewed a series of retrieved acetabular liners with a fracture of the superior rim to assess the factors that played a role in their failure. Methods: Four Longevity acetabular bearings, which had been retrieved from two patients after seven to twenty-seven months in vivo, were visually examined for clinical damage, were assessed with use of Fourier transform infrared spectroscopy to determine the level of oxidation, and were analyzed for mechanical properties and fracture surface characterization. Control data were obtained from never-implanted devices and from global reference ultrahigh molecular weight polyethylene bar stock as an industry calibration material. Results: All four retrieved liners demonstrated articular surface wear modes, which in most cases were rated as moderate, and none were rated as severe. All showed cracking or rim failure of the liner at the superior aspect along the groove in the polyethylene that engages the locking ring of the shell. The retrieved liners had no measurable oxidation, and the mechanical properties were comparable with those of never-implanted material. Conclusions: There was no notable in vivo degradation of the retrieved liners. Important factors related to failure appear to be thin polyethylene at the cup rim, relatively vertical cup alignment, and the material properties of the highly cross-linked polyethylene that are decreased relative to conventional polyethylene. The critical dimension with respect to rim failure in modular liners appears to be the minimum thickness at the equatorial region. Clinical Relevance: For a given implant design and loading, highly cross-linked polyethylene may be more susceptible to fatigue damage, such as rim cracking, than is conventional polyethylene. The potential for excess rim loading on thin polyethylene should be assessed carefully when the use of a cross-linked liner and a large femoral head is being considered, particularly in a cup with a more vertical abduction angle.
1 August 2007 in The Journal of Arthroplasty
1 October 2010 in Journal of Bone and Joint Surgery
Series of retrieved remelted highly cross-linked ultra-high molecular weight polyethylene bearings from a number of device manufacturers and (2) compared the retrieval results with findings for shelf-stored control specimens. The hypothesis was that radiation-cross-linked remelted ultra-high molecular weight polyethylene would maintain oxidative stability in vivo comparable with the stability during shelf storage and in published laboratory aging tests. Methods: Fifty remelted highly cross-linked ultra-high molecular weight polyethylene acetabular liners and nineteen remelted highly cross-linked ultra-high molecular weight polyethylene tibial inserts were received after retrieval from twenty-one surgeons from across the U.S. Thirty-two of the retrievals had been in vivo for two years or more. Each was measured for oxidation with use of Fourier transform infrared spectroscopy. A control series of remelted highly cross-linked ultra-high molecular weight polyethylene acetabular liners from three manufacturers was analyzed with electron paramagnetic resonance spectroscopy to measure free radical content and with Fourier transform infrared spectroscopy to measure oxidation initially and after eight to nine years of shelf storage in air. Results: The never-implanted, shelf-aged controls had no measurable free-radical content initially or after eight to nine years of shelf storage. The never-implanted controls showed no increase in oxidation during shelf storage. Oxidation measurements showed measurable oxidation in 22% of the retrieved remelted highly cross-linked liners and inserts after an average of two years in vivo. Conclusions: Because never-implanted remelted highly cross-linked ultra-high molecular weight polyethylene materials had no measurable free-radical concentration and no increase in oxidation during shelf storage, these materials were expected to be oxidation-resistant in vivo. However, some remelted highly cross-linked ultra-high molecular weight polyethylene retrievals showed measurable oxidation after an average of more than two years in vivo. This apparent departure from widely expected behavior requires continued study of the process of in vivo oxidation of ultra-high molecular weight polyethylene materials. Clinical Relevance: Remelted highly cross-linked ultra-high molecular weight polyethylene acetabular and tibial retrievals showed unexpected oxidation....
1 August 2012 in The Journal of Arthroplasty
JCJ. Caitlin Huot Carlson