The development of energy storage devices encourages the sustainability of research on basic materials of supercapacitor technology. SrTiO3 is one of metal oxide called as titanate alkali metal ATiO3 (A = Ba, Sr, Ca). This material shows an excellent dielectric constant, thus expected to be potential as raw material of supercapacitor. In this work, boron was used as a dopant on the SrTiO3 system to modify its local structure and enhance the electrical properties. Synthesis SrTi1-xBxO3 was carried out using a solid-state reaction method followed by the sintering process in various molar ratio. The microstructure of SrTi1-xBxO3 compound was identified by X-ray Diffraction with Cu-Kα. XRD pattern identified the presence of SrTi1-xBxO3 phase with a slight change in the lattice parameters. I-V measurement confirmed that the electrical conductivity increased gradually up to 16.04 Ω-1cm-1. For investigating their application for electrode materials, CV was employed and it presents that the specific capacitance and energy density of x = 0.08 were 5.488 Fg-1 and 0.110 Jg-1.
1 May 2018 in IOP Conference Series: Materials Science and Engineering
Co0.5Ni0.5Fe2O4 magnetic nanoparticles have been successfully synthesized by coprecipitation method with varying synthesis temperature and NaOH concentration. X-ray diffraction (XRD) analysis confirmed that Co0.5Ni0.5Fe2O4 nanoparticles have spinel cubic crystal structure. The particle size of the sample synthesized at 3 M NaOH was 7.3 nm and then increased with the increase of NaOH concentration. It is caused by the increase of particle growth rate. The particle size of the sample synthesized at 30 °C was 10.2 nm and then increased with the increase of temperature. The lattice parameter of the sample was constant at 8.5 Å with varying synthesis temperature and NaOH concentration. The maximum magnetization and the coercivity of the sample synthesized at 3 M NaOH was 11.3 emug-1 and 0.1 kOe, respectively, and then increased with the increase of NaOH concentration. It is caused by the increase of crystallite size in a single domain. The maximum magnetization and the coercivity of the sample synthesized at 30 °C was 9.9 emug-1 and 0.1 kOe, respectively, and then increased with the increase of temperature. Transmission Electron Microscopy (TEM) image showed that the sample was agglomerated. Selective Area Electron Diffraction (SAED) image shows that sample is confirmed peak is appearing in XRD. The Fourier Transform Infra-Red (FTIR) spectra confirmed that vibration of octahedral and tetrahedral metal-oxide bond is 601.8 cm-1 and 370.3 cm-1. The purpose of this work is to investigate the effect of synthesis temperature and NaOH concentration on the relation between crystal structure and magnetic properties.
Cobalt substituted nickel ferrite nanoparticles (Ni1-xCoxFe2O4) with stoichiometric proportion (x) from 0.2 to 0.8 have been synthesized by co-precipitation method with synthesis temperature of 90°C. The crystallite size of Ni1-xCoxFe2O4 nanoparticles were within range of 14 – 27 nm. The X-ray diffraction (XRD) analysis informed that the lattice parameter of Ni1-xCoxFe2O4 nanoparticles at x = 0.3 was 8.423 Å, and then increased with increasing Co concentration. This is due to substitution of larger ionic radius of Co2+. The selected area electron diffraction (SAED) patterns showed that increasing Co concentration exhibited more prominent ring indicating well crystallinity. It could be confirmed from the crystallinity of the sample for x = 0.7 was higher than 0.5. The SAED patterns of Ni1-xCoxFe2O4 nanoparticles also displayed polycrystalline diffraction ring. The fourier transform infrared spectroscopy (FTIR) spectra of Ni1-xCoxFe2O4 showed the presence of vibration bands of metal ions within the range of 370.33 cm−1 – 601.79 cm−1 at the tetrahedral and octahedral sites, respectively. These two bands indicated the formation of a spinel ferrite structure. The magnetic hysteresis results showed that the maximum magnetization at 15 kOe of Ni1-xCoxFe2O4 nanoparticles at x = 0.2 was 7.0 emu/g, and then increase to 29.0 emu/g at x = 0.8 with increasing Co concentration. The results could be attributed to substitution of higher magnetic moment of Co2+. The coercivity (Hc) of Ni1-xCoxFe2O4 nanoparticles at x = 0.2 was 59.4 Oe, and then increase to 641.75 Oe at x = 0.6 with increasing Co concentration. This is due to cobalt having higher magnetic anisotropy than nickel.
19 November 2018 in IOP Conference Series: Materials Science and Engineering
Co0.8Ni0.2Fe2O4 nanoparticles were synthesized by coprecipitation method and annealed at different temperatures (200, 400, 600, 800 and 1000 °C). The X-ray diffraction (XRD) exhibited the formation of spinel cubic structure. The crystallite size of Co 0.8Ni0.2Fe2O4 nanoparticles at the annealing temperature of 200 °C was 7.0 nm and then increased with the increase of annealing temperature. The reason for this is that the particles grow faster and larger at a higher temperature. The transmission electron microscopy (TEM) images showed that the size distribution of the particles was increased with the increase of annealing temperature. It was also seen from the samples that most of the particles appeared nearly spherical in shape with slight agglomeration, particularly at higher annealing temperature. The Fourier transform infrared spectroscopy (FTIR) spectra of Co0.8Ni0.2Fe2O4 nanoparticles confirmed the presence of vibration bands of metal ions at 370.30-401.9 cm-1 and 586.36-601.79 cm-1 which was in a region of octahedral and tetrahedral sites, respectively. The values of the gap energy of Co0.8Ni0.2Fe2O4 nanoparticles observed ultraviolet-visible (UV-Vis) spectroscopy were in the range of 4.25-4.94 eV. The gap energy was decreased with the increase of annealing temperature and the increase of crystallite size.