The process variant of friction surfacing (FS) depositing multiple layers on top of each other is known as multi-layer friction surfacing (MLFS). Due to the solid-state nature of the process, re-heating is significantly reduced compared to common fusion-based AM techniques. The work gives a detailed and fundamental insight into the microstructure along the MLFS build direction for two different aluminum alloys and different process parameters. Focusing on the grain size distribution and recrystallization ratio, the stacks show a higher degree of recrystallization and finer grains at the interfaces. The observed grain sizes at the interfaces were 2.0 µm (AA5083) and 1.1 µm (AA2024), and 5.8 µm (AA5083) and 3.1 µm (AA2024) at the layer center. For the non-precipitation-hardenable alloy (AA5083), the local microstructural trend could be related to the hardness distribution along the stacks, i.e., a slightly higher hardness at the layer interfaces (95 HV) compared to the layer center (90 HV). The relationship is more complex for precipitation-hardenable alloys (AA2024), which show a rise in hardness between 40 HV0.2 and 45 HV0.2 along the stack height. The effect of subsequent layer depositions on the microstructure and hardness is discussed and a distinctive grain size distribution along the build direction was shown to be a fundamental characteristic.
Solid-state additive manufacturing (AM) processes such as multi-layer friction surfacing (MLFS) can overcome typical disadvantages of fusion-based AM such as high residual stresses, porosity or hot cracking. The tool-less process setup of MLFS prevents contamination of the resulting components, e.g., caused by wear or the use of lubricants. The present study investigates MLFS for the precipitation-hardenable alloy AA2024-T3 using a process parameter that yields a high build rate relevant for industrial applications. The fatigue performance is shown and the microstructural and the mechanical anisotropy is examined. The fatigue properties in deposition direction show a high cycle fatigue limit of 170.5 MPa and a decrease in the maximum stress level compared to the base material due to precipitate overageing. The microstructure shows a Brass $$\{011\}\langle 211\rangle$$ texture at the bottom of the layers due to the application of high axial forces. In the center of the layer, no preferred texture was observed, while $$\text {B}\{\bar{1}12\}\langle 110\rangle$$ / $$\bar{\text {B}}\{1\bar{1}\bar{2}\}\langle \bar{1}\bar{1}0\rangle$$ shear textures were observed at the top part of the deposited layers. An elongated grain morphology with aspect ratios above 2 is present over the entire layer height. These microstructural characteristics cause anisotropy in mechanical properties, with highest ultimate tensile strength and elongation in deposition direction, i.e., 408 ± 5 MPa and 18 ± 3 % respectively, and the lowest values along the build direction, i.e., 377 ± 21 MPa and 9 ± 3 % respectively. The observed behavior is of considerable importance for the industrial design and application of components manufactured with MLFS as they show that MLFS can also result in anisotropic material properties, depending on the chosen process parameters. It requires careful selection of the right combination of stud material and process parameters to achieve isotropic properties in the deposited structure.