For (V
1−
x Al x )
1−
y N y an extensive and theoretically unexplained spread in experimentally obtained elastic moduli ranging from 254 to 599 GPa is reported in literature. To identify its origin, the effect of chemical composition (0 ⩽ x ⩽ 0.75), non-metal to metal ratio (N/M-ratio: 0.48 ⩽ y ⩽ 0.52), and stress state (−6 ⩽ σ ⩽ 2 GPa) on the elastic modulus at room temperature is studied sytematically by density functional theory employing the Debye–Grüneisen model. As the Al concentration is increased from x = 0 to x = 0.75, strong Al–N sp 3 d 2 hybridization causes an increase in elastic modulus of 26%. The effect of the N/M-ratio on the elastic properties is also Al content dependent. As y is increased from y = 0.50 to y = 0.52, decreasing bond distance upon vacancy formation causes an anomalous increase in the elastic modulus of 6% for V
1−
y N y , while a decrease in elastic modulus of up to 5% occurs for (V
1−
x Al x )
1−
y N y . A stress state variation from +2 to −6 GPa increases the elastic modulus e.g. for (V 0.5 Al 0.5 ) 0.5 N 0.5 by 70 GPa and hence 13% due to shifts in density of states towards lower energies implying bond strengthening. Thus, it is suggested that the extensive spread of 58% in reported elastic moduli for (V
1−
x Al x )
1−
y N y can at least in part be rationalized based on variations in chemical composition, off-stoichiometry induced point defects, and stress state.
21 August 2024 in Journal of Vacuum Science & Technology A
A comparative study on nonreactively direct current magnetron sputtered (DCMS) and high-power pulsed magnetron sputtered (HPPMS) MoSi2-based coatings has been implemented with the objective of advancing the knowledge on the growth conditions and oxidation resistance of MoSi2 thin films. The energy supplied during the growth process (i.e., deposition temperature and ionization degree) exerts a significant influence on the phase formation and morphology. At 200 °C, highly dense but x-ray amorphous films are prevalent, whereas an increase up to 400 °C leads to dense and fine-columnar structured hexagonal MoSi2 films. Increased growth temperatures (≥500 °C for DCMS) and strongly ionized plasma states result in the formation of dual-phase structures (h-MoSi2 and t-Mo5Si3), accompanied by slightly underdense but strongly columnar grains. The MoSi1.92 HPPMS film (1000 Hz, 10% duty cycle) grown at 500 °C exhibits the maximum hardness of 22.8 GPa and an elastic modulus of approximately 400 GPa. In long-term oxidation tests conducted at 600, 850, and 1200 °C (up to 100 h), all MoSi2-based films exhibited a temperature-dependent scale formation. Up to 850 °C, the formation of a continuous, dense protective scale is disrupted by the competing growth of MoOx and SiOx. At temperatures exceeding 1200 °C, all MoSi2-based coatings analyzed demonstrate exceptional oxidation resistance, resulting in the formation of a continuous, dense SiO2 scale. At 1500 °C for 30 min, the initially slightly underdense and dual-phased MoSi1.92 coating achieved a scale thickness of only 670 nm, thereby demonstrating the exceptional oxidation resistance capabilities of HPPMS-grown MoSi2-based coatings.
27 October 2023 in Journal of Vacuum Science & Technology A
A combination of time-averaged mass spectroscopy (MS), time-averaged optical emission spectroscopy (OES), and plasma transport modeling was employed to understand the transport processes of ions and atoms in high-power impulse magnetron sputtering discharges resulting in changes in the stoichiometry of NbCx films during their deposition from a stoichiometric NbC compound target at different repetition frequencies and duty cycles. Mass spectrometry showed that the fluxes of ions originating from the elements of the target increase with increasing pulse power density (and decreasing pulse length) due to an increasing electron density and, thus, electron-impact ionization probability. Due to the higher ionization energy and much lower ionization cross section of C (compared to Nb), it was found that the contribution of C+ ions to the deposition flux is practically negligible. Additionally, OES tracked the densities of ions and atoms at different distances from the target. The OES analysis revealed that the atom densities decreased as the pulse power density increased. In contrast, the ion densities exhibited an increase, which is consistent with the findings of MS. Using the data from MS, OES, and modeling, we were able to estimate the fluxes of atoms to the substrate. Our observations demonstrated a transition from C-rich toward Nb-rich flux of film-forming species with increasing pulse power density, corresponding to changes in the film composition. We further discuss the role of internal plasma processes that are responsible for this transition.