Valve metals such as titanium (Ti), zirconium (Zr), niobium (Nb) and tantalum (Ta) that confer a stable oxide layer on their surfaces are commonly used as implant materials or alloying elements for titanium-based implants, due to their exceptional high corrosion resistance and excellent biocompatibility. The aim of this study was to investigate the bioactivity of the nanostructures of tantala (Ta2O5), niobia (Nb2O5), zirconia (ZrO2) and titania (TiO2) in accordance to their roughness and wettability. Therefore, four kinds of metal oxide nanoporous and nanotubular Ta2O5, Nb2O5, ZrO2 and TiO2 were fabricated via anodization. The nanosize distribution, morphology and the physical and chemical properties of the nanolayers and their surface energies and bioactivities were investigated using SEM-EDS, X-ray diffraction (XRD) analysis and 3D profilometer. It was found that the nanoporous Ta2O5 exhibited an irregular porous structure, high roughness and high surface energy as compared to bare tantalum metal; and exhibited the most superior bioactivity after annealing among the four kinds of nanoporous structures. The nanoporous Nb2O5 showed a uniform porous structure and low roughness, but no bioactivity before annealing. Overall, the nanoporous and nanotubular layers of Ta2O5, Nb2O5, ZrO2 and TiO2 demonstrated promising potential for enhanced bioactivity to improve their biomedical application alone or to improve the usage in other biocompatible metal implants.
4 November 2013 in Journal of Materials Chemistry B
Titanium and its alloys are able to grow a stable oxide layer on their surfaces and have been used frequently as substrates for anodization in an electrochemical surface treatment. A nanotubular oxide layer is formed in the presence of fluorine anion (F−) via anodization due to the competition between oxide formation and solvatization. In this study, a highly ordered titania–zirconia–zirconium titanate (TiO2–ZrO2–ZrTiO4) nanotubular layer was formed on the surface of Ti50Zr alloy via anodic oxidation in an F− containing electrolyte. The sizes of the nanotubes (i.e., the inner and outer diameters, and wall thicknesses), morphology, crystal structure, hydrophilic properties and components of the TiO2–ZrO2–ZrTiO4 nanotubular layer before and after annealing were examined by scanning electron microscopy (SEM), thin film X-ray diffraction, X-ray photoelectron spectroscopy (XPS) analysis and water contact angle measurements. The results indicated that the inner diameter, outer diameter and wall thickness of the as-formed TiO2–ZrO2–ZrTiO4 nanotubes were distributed in the ranges of 3–120 nm, 12–165 nm and 3–32 nm, respectively, and depended on the F− concentration of the electrolyte and the applied potential during anodization. The number of smaller nanotubes increased with increasing F− concentration and the mean nanotube inner and outer diameters increased with increasing applied potential. The as-formed TiO2 and ZrTiO4 nanotubes exhibited an amorphous structure and the as-formed ZrO2 nanotubes displayed an orthorhombic structure. These phases transformed into anatase TiO2 and orthorhombic ZrO2 and ZrTiO4 after annealing. The hydrophilic properties of the TiO2–ZrO2–ZrTiO4 nanotubular layer were affected by the size distribution of the nanotubes. The surface roughnesses and the nanotubular character transformed the nanotubes to exhibit superhydrophilic properties after annealing. The TiO2–ZrO2–ZrTiO4 nanotubular surface on Ti50Zr alloy exhibited higher surface energy than that of the TiO2 nanotubular surface on commercially pure (CP) titanium.
Cell adhesion on the TiO 2 –ZrO 2 –ZrTiO 4 nanotubes fabricated via anodization using a non-aqueous electrolyte was significantly influenced by the nanoscale topographical parameters.