Reducible supports can affect the performance of metal catalysts by the formation of suboxide overlayers upon reduction, a process referred to as the strong metal–support interaction (SMSI). A combination of operando electron microscopy and vibrational spectroscopy revealed that thin TiO x overlayers formed on nickel/titanium dioxide catalysts during 400°C reduction were completely removed under carbon dioxide hydrogenation conditions. Conversely, after 600°C reduction, exposure to carbon dioxide hydrogenation reaction conditions led to only partial reexposure of nickel, forming interfacial sites in contact with TiO x and favoring carbon–carbon coupling by providing a carbon species reservoir. Our findings challenge the conventional understanding of SMSIs and call for more-detailed operando investigations of nanocatalysts at the single-particle level to revisit static models of structure-activity relationships.
Thermal pyrolysis is gaining industrial adoption to convert large volumes of plastic waste into hydrocarbon feedstock. However, it suffers from a high reaction temperature and relatively low selectivity. Utilizing a catalyst in the process, moving from thermal pyrolysis to catalytic cracking could help overcome both challenges. In order to develop efficient catalyst materials for this process, understanding structure-composition-performance relationships is critical. In this work, we show that in contrast to cracking of small molecules, plastic cracking activity using ultrastable zeolite Y materials does not depend on the bulk Brønsted acid site content, but rather on the concentration of acid sites located on the outer surface and in mesopores. This external acidity, however, fails to capture all the observed performance trends. Detailed kinetic experiments reveal that the scaling of the reaction rate with the catalyst loading differs drastically between highly similar catalyst materials. More specifically, doubling the catalyst loading leads to doubling of the reaction rate for one material, while for another it leads to more than fivefold increase. When very bulky reactants, such as polyolefins, are converted over microporous catalysts, structure-composition-performance relationships established for smaller molecules need to be revisited.
The process of hydrodesulfurization is one of the most important heterogeneous catalytic reactions in industry as it helps with reducing global SOx emissions by selectively removing the sulfur contaminants from commercial fuel. In this work, we successfully combine high-pressure scanning tunneling microscopy and reaction modeling using density functional theory to observe the hydrodesulfurization of methanethiol (CH3SH) on the Co-substituted S edges of a Co-promoted MoS2 model catalyst in situ at near-industrial conditions and investigate the plausible reaction pathways. The active sites on the Co-substituted S edges show a time-varying atomic structure influenced by the hydrodesulfurization reaction rate. The involvement of the edge Co site allows for the C-S bond scission to occur at appreciable rates, and is the critical step in the hydrodesulfurization of CH3SH. The atomic structures of the S-edge active sites from our reaction models match excellently with those observed in situ in the experiments.
Understanding catalytic processes requires insights into the behavior of reactants, intermediates, and products at the surface of a solid catalyst. This is often studied via in situ or operando vibrational spectroscopy and by theoretical calculations. However, direct comparison between experimental and theoretical vibrational frequencies remains challenging and requires careful methodological treatment. Here, we present a systematic computational framework for calculating and scaling the fundamental vibrational frequencies of fourteen key intermediates involved in catalytic C 1 reactions over nickel. Such intermediates were modeled on Ni(111), Ni(100), Ni(110), and Ni(211) crystal surfaces. Multiple density functional theory (DFT) methods and basis sets were benchmarked. Linear scaling equation (LSE) correction was applied to all computed wavenumbers. The result is a validated database of LSE‐corrected vibrational frequencies, designed to aid experimentalists in infrared (IR) spectral interpretation. We illustrate its application with a phenomenological evaluation of the CO adsorption region, comparing calculated spectra to IR spectra from CO 2 methanation over four Ni/SiO 2 catalysts. For this analysis, we used a dual‐model approach, computing CO ∗ frequencies on both extended facets and a 1.439 nm Wulff‐constructed nanoparticle to account for size‐dependent effects. The analysis highlights how adsorption site and adsorbate interactions influence vibrational features, underscoring the need for both more complex models and complementary experiments to accurately capture effects, such as peak shifts, inhomogeneous broadening, and intensity transfer that govern the spectra of working catalyst surfaces.
The Front Cover illustrates the integration of density functional theory (DFT) and operando infrared spectroscopy in catalytic C1 chemistry over nickel metal nanoparticles. A systematic framework for scaling the computed vibrational frequencies of key intermediates across structurally distinct surfaces supports spectral assignment and comparison with experiment. Further details are provided in the Research Article by B. M. Weckhuysen and co-workers (DOI: 10.1002/ceur.202500338). Artwork by Dr. Ellen B. Sterk.