The electrodeposition of Cu2O thin films was systematically investigated by varying the chloride ion (Cl−) concentration in the electrolyte. Current-time transient analysis revealed an increase in the diffusion coefficient (D₀) from 2.09 × 10−7 cm2 s−1 at low Cl− concentration to 3.72 × 10−6 cm2 s−1 at higher Cl− levels, indicating enhanced mass transport and faster growth kinetics. Dimensionless current-time transients compared with the Scharifker-Hills model confirmed progressive nucleation across all conditions, with a decreasing nucleation rate (AN₀) from 21.685 × 106 cm−2 s−1 to 4.790 × 106 cm−2 s−1 as Cl− concentration increased. Similarly, the saturation nucleation density (Nsat) declined from 16.980 × 106 cm−2 to 4.847 × 106 cm−2, suggesting that higher Cl− concentrations favor larger grain formation by reducing the density of active nucleation sites. X-ray diffraction analysis confirmed the formation of single-phase cubic Cu2O with a dominant (111) orientation across all samples, with crystallite sizes increasing from 62 nm to 94 nm as Cl− concentration increased. These findings highlight the crucial role of electrolyte composition in controlling the nucleation and growth mechanisms of Cu2O films, offering valuable insights for optimizing deposition parameters in optoelectronic and energy applications.
1 July 2025 in Journal of the Electrochemical Society
This work investigates the impact of zinc acetate (ZnAc) precursor concentration on the electrochemical and photocatalytic performance of ZnO thin films synthesized via chemical solution deposition. Electrochemical impedance spectroscopy (EIS) and Mott-Schottky analysis revealed that increasing ZnAc concentration from 0.2 to 0.8 M significantly reduced charge transfer resistance and enhanced carrier density. The film prepared with 0.8 M ZnAc exhibited the lowest Rct (0.19 kΩ), highest double-layer capacitance (88.7 μF), and fastest interfacial charge transfer, indicating superior electrochemical behavior. Photocatalytic activity was evaluated using Rhodamine B (RhB) degradation under UV light. The ZnO-0.8 M film showed the most efficient degradation rate, with absorbance measurements confirming a continuous decrease in RhB concentration over time. The degradation mechanism was attributed to the generation of reactive oxygen species (·OH and ·O2−) through UV-induced electron-hole pair excitation in ZnO, leading to oxidative decomposition of RhB into environmentally benign products. The structural properties and optimized charge transport of the ZnO-0.8 M film underlie its superior performance. These findings highlight the critical role of precursor concentration in tailoring ZnO thin film properties for advanced photoelectrochemical and photocatalytic applications.
1 June 2025 in Journal of the Electrochemical Society
This study investigates the electrodeposition of Cu₂O thin films on fluorine-doped tin oxide substrates, focusing on the effects of deposition time on their structural, optical, and electrochemical properties. The electrochemical characterization led to insights into the nucleation and growth mechanisms of Cu2O, as identified through cyclic voltammetry and chronoamperometry. X-ray diffraction analysis confirmed the formation of cubic Cu2O, revealing a preferential (111) orientation, particularly prominent at longer deposition times. Optical studies indicated a decrease in the bandgap energy from 2.33 to 2.21 eV with increasing deposition time, attributed to improved crystallinity and the introduction of defect states. Atomic force microscopy showed that surface roughness increased from 17.23 to 26.025 nm as deposition time extended from 300 to 1200 s. Furthermore, electrochemical impedance spectroscopy demonstrated enhanced charge transfer capabilities, with a reduction in charge transfer resistance (Rct) from 2.96 to 1.14 × 103 Ω·cm2, highlighting the impact of deposition time on the electrochemical performance of the thin films.
3 February 2026 in Journal of the Electrochemical Society
N-Type Cu 2 O is a promising photocatalyst due to its direct bandgap, enabling strong visible-light absorption. When used as a photoelectrode, however, its performance depends critically on film thickness, which must balance light absorption with efficient charge transport. This study systematically optimized the thickness of electrodeposited Cu 2 O films on FTO substrates by varying deposition time from 5 to 40 min. As deposition time increased, the films evolved from pyramidal nanostructures to dense polycrystalline layers, with thicknesses ranging from ~150 nm to ~1200 nm. Thicker films exhibited improved visible-light absorption and a slight bandgap narrowing from 2.35 to 2.25 eV. All samples showed stable anodic photocurrents characteristic of n-type behavior. The highest photocurrent 0.118 mA occurred for the film deposited for 30 min, corresponding to an optimal thickness of ~750 nm. At this thickness, the film effectively absorbs incident photons while still allowing photogenerated carriers to reach the interface before recombining. Beyond this optimal point, photocatalytic activity declined sharply despite continued gains in light absorption, due to the thickness exceeding the charge-carrier diffusion length, which increased recombination and transport resistance. These results highlight the importance of precise thickness control for maximizing Cu 2 O/FTO photoanode efficiency.