Solid oxide fuel cells (SOFCs) are efficient combined heat and power devices that can flexibly operate on a variety of fuels, such as H 2 , CO, or hydrocarbons. Shifting to these alternative fuels as a primary energy source can contribute significantly to the decarbonization of the energy sector, as electrochemical oxidation of these fuels produces H 2 O and capture-ready CO 2 . Additionally, power production from hydrocarbons, for example, could serve as an effective approach to allow for continued development of the oil and gas sector, while still achieving significantly reduced emissions during energy production. The long-term stability of SOFCs is still a major challenge that is hindering widespread commercialization. The prominent reason for this is the high operating temperatures, which greatly accelerate degradation phenomena. Particle sintering, phase segregation, cation migration, and microstructural changes are some of the major challenges to overcome when it comes to electrode design. 1,2,3 Traditional anode materials currently employed in SOFC systems are composite cermets, such as Ni- yttria-stabilized zirconia or Ni- gadolinium-doped ceria. 4,5 These materials are well known for suffering deactivation due to the aforementioned causes of degradation, including morphology change, carbon deposition in hydrocarbon fuels and sulfur poisoning. 6 Therefore, perovskite systems, such as La-based La x A 1-x BO 3-δ (A = Sr, Zr, Y; B = Cr, Fe, Ni, Co, Mn), have emerged as next generation anode materials due to their high redox stability at intermediate and high operating temperatures (500-800 o C). 7,8,9,10 Our group has been developing and modifying a perovskite oxide (ABO 3 ) catalyst with the specific formula of La 0.3 Ca 0.7 Fe 0.7 Cr 0.3-x M x O 3-δ (M = Ni, Co, Cu). Investigations of this material and its analogue, La 0.3 Sr 0.7 Fe 0.7 Cr 0.3 O 3-δ , have established a stability window in mixtures of CO 2 -CO, showing that the perovskite phase remains intact under a pO 2 window of 0.21-10 -21 atm. 11 Consistent with this, these catalysts have displayed high activity towards many reactions, such as H 2 oxidation, steam reduction, oxygen reduction, oxygen evolution, CO oxidation, and CO 2 reduction. 11,12,13,14 Further enhancement in conversion kinetics has been achieved by decorating the catalyst surface with transition metal nanoparticles (NPs) though exsolution. For example, we have demonstrated that exsolved Ni NPs can enhance the kinetics of CO 2 reduction at 800 o C by ~15% and CO oxidation by ~75%. In addition, these NPs display no carbon formation in 90:10 CO:CO 2 for 25 hours at 800 o C. 15 Here, we have expanded on prior work with La 0.3 Ca 0.7 Fe 0.7 Cr 0.3-x Ni x O 3-δ (LCFCrNi) and its parent materials by studying the long-term performance and durability in a simulated 100% fully reformed gas mixture of 1:2 CH 4 :H 2 O, which would generate 4:1 H 2 :CO 2 upon complete steam methane reforming. Material phase, morphology, and structure changes as a function of long-term constant current experiments are also being explored. LCFCr and its doped analogues were prepared by combustion synthesis and characterized by SEM/EDX, TEM, and XRD, to confirm morphology, crystal structure, and composition as a function of temperature and gas environment. 15 Symmetrical electrolyte-supported SOFCs were constructed using our catalyst, with LCFCrNi at the anode (0.5 cm 2 ) and LCFCr at the cathode (1 cm 2 ), with the catalyst layers screen-printed on both sides of a samaria-doped ceria (SDC)-buffered scandia-stabilized zirconia (ScSZ) electrolyte (ca. 150 μm). This was followed by sintering at 1100 °C for 2 h in air, with porous Au current collectors used. Electrochemical evaluation was conducted at 800 o C under 4:1 H 2 :CO 2 with the gas flow rates and composition controlled by mass flow controllers. Under both open circuit and polarized conditions, durability was measured in-situ for 100-250 h, with electrochemical impedance spectroscopy carried out every 20 h to track changes in resistance and capacitance. Additionally, gas analysis was carried out by on-line mass spectrometry to verify outlet gas composition and fuel utilization. Figure 1a shows the current-voltage data obtained from a SOFC with a LCFCrNi anode in 4:1 H 2 :CO 2 and 4:1 H 2 :N 2 at 800 °C. Under 4:1 H 2 :N 2 , a maximum power density of 0.43 W/cm 2 was achieved at 0.92 A/cm 2 (0.20 V overpotential vs. LCFCr reference in air). The reformed gas mixture (4:1 H 2 :CO 2 ) has a 22% lower performance, achieving a maximum power output of 0.35 W/cm 2 at the same overpotential. This is explained by the reverse water-gas shift reaction producing CO, which could have more sluggish oxidation kinetics compared to H 2 . 16 Reverse water-gas shift reaction also consumes H2 to produce H2O, thereby decreasing the H2 concentration at the anode. The OCV in 4:1 H 2 :CO 2 is ca 1.0 V and significantly lower than the OCV value of 1.15 V in 4:1 H 2 :N 2 at 800 °C. The difference in OCV values suggests that pO2 in 4:1 H 2 :CO 2 is significantly higher than in 4:1 H 2 :N 2 , thereby reducing the driving force. Chronopotentiometry experiments were carried out at 0.35 A/cm 2 at an anode overpotential of 0.16 V (vs. a LCFCr reference electrode placed on the cathode side of the button cell) to analyze the durability of the SOFC in 4:1 H 2 :CO 2 . Biased EIS data were acquired every 20 hours to track changes in the resistors and capacitors, revealing that Rs increased from 0.37 to 0.41 Ω cm 2 (14% increase), while Rp increased from 0.52 to 0.67 Ω cm 2 (29% increase), occurring predominantly in the low-frequency arc, while the capacitance of the low frequency arc was not observed to change. Initial investigations into the causes of the observed degradation have highlighted the porous Au current collectors as the primary source of degradation due to the observed increase in Rs. Post-mortem analysis was performed on both the anode and cathode by SEM to investigate if any structural and morphological changes occurred after 100 h. Figure 1b shows the full cross-section of one button cell, showing the current collector, electrode, buffer and electrolyte layers and their corresponding thicknesses and microstructure. Here, we utilized a ca. 20 µm thick anode and 30 µm thick cathode, both with particle sizes of ca. 1-2 µm and a porosity estimated to be 50%. Higher magnification images of the anode and cathode are shown in Figures 2a-d. The cathode, imaged near the SDC buffer layer (Figure 2a-b), is observed to maintain high quality LCFCr/Au and LCFCr/SDC interfaces, with smooth surfaces and no structural or morphological changes occurring after 100 h of oxygen reduction. The anode surface (Figure 2c-d) also shows high quality LCFCrNi/Au and LCFCrNi/SDC interfaces, with no signs of delamination. After pre-reduction at 800 o C for 2 h under 5% H 2 /95% N 2 , the anode surface undergoes significant re-crystallization, appearing as surface roughening. Additionally, NPs are observed to cover the surface, appearing predominantly hemispherical, ca. 60 nm in size, and distributed homogeneously across grains without a preference for exsolution at grain boundaries. Notably, NP coverage is observed throughout the entire thickness of the anode, although some regions showed much higher population densities. The surface roughening appears identical as compared to a reference LCFCrNi sample that was pre-reduced for 2 h under 5% H 2 /95% N 2 at 800 o C but not exposed to 4:1 H 2 :CO 2. Hence, re-crystallization likely only occurs under highly reducing conditions, as this was not observed for the cathode. Further analysis of the NPs by TEM, on a LCFCrNi powder sample pre-reduced under the same conditions described above for the anode (Figure 2g), revealed that, after 2 hours of reduction, the NPs formed are highly amorphous and are composed of 98% Ni - 2% Fe. Comparison of the average NP population density, diameter, and crystallinity between the anode and the pre-reduced reference LCFCrNi (Figures 2c-d and 2e-f) suggests that, for mixed conductors such as LCFCrNi, which readily undergo exsolution, anodic polarization effectively prevents NP growth, as metal reduction can not occur under these conditions. Another notable observation is the enrichment of Fe and Ni NPs seen at the Au current collector/LCFCrNi interface, which is still not fully understood. This may not be a negative feature, as this may enhance the quality of interfacial bonding. Upon cooling to room temperature under flowing 4:1 H 2 :CO 2 , NiO and Fe 2 O 3 are detected on the surface of the Au current collector surface by EDX. Other work includes determining the effect of different pre-reduction (exsolution) and operating conditions, including gas composition, temperature, and operating current, on exsolved metal NP size and distribution, as well as electrochemical performance and durability. Acknowledgements The authors acknowledge Mykhailo Pidburtnyi for helpful discussions regarding the interpretation of results. Additionally, we recognize Occam’s Technologies, Precision Drilling, and the Natural Sciences and Engineering Research Council of Canada (NSERC) for financial support of this work. References Zarabi Golkhatmi, S.; Asghar, M. I.; Lund, P. D. A Review on Solid Oxide Fuel Cell Durability: Latest Progress, Mechanisms, and Study Tools. Renewable and Sustainable Energy Reviews 2022 , 161, 112339. DOI:10.1016/j.rser.2022.112339. Mehran, M. T.; Khan, M. Z.; Song, R.-H.; Lim, T.-H.; Naqvi, M.; Raza, R.; Zhu, B.; Hanif, M. B. A Comprehensive Review on Durability Improvement of Solid Oxide Fuel Cells for Commercial Stationary Power Generation Systems. Applied Energy 2023 , 352, 121864. DOI:10.1016/j.apenergy.2023.121864. Mahato, N.; Banerjee, A.; Gupta, A.; Omar, S.; Balani, K. Progress in Material Selection for Solid Oxide Fuel Cell Technology: A Review. Progress in Materials Science 2015 , 72, 141–337. DOI:10.1016/j.pmatsci.2015.01.001. Shao, X.; Budiman, R. A.; Sato, T.; Yamaguchi, M.; Kawada, T.; Yashiro, K. Review of Factors Affecting the Performance Degradation of Ni-Ysz Fuel Electrodes in Solid Oxide Electrolyzer Cells. Journal of Power Sources 2024 , 609, 234651. DOI:10.1016/j.jpowsour.2024.234651. Ahmed, N.; Devi, S.; Dar, M. A.; Ibrahim, S. K.; Sharma, A.; Sharma, N.; Paul, S.; Ahamed, S. R. Anode Material for Solid Oxide Fuel Cell: A Review. Indian Journal of Physics 2023 , 98 (3), 877–888. DOI:10.1007/s12648-023-02860-3. Christensen, K. O.; Chen, D.; Lødeng, R.; Holmen, A. Effect of Supports and Ni Crystal Size on Carbon Formation and Sintering during Steam Methane Reforming. Applied Catalysis A: General 2006 , 314 (1), 9–22. DOI:10.1016/j.apcata.2006.07.028. Jiang, S. P. Development of Lanthanum Strontium Cobalt Ferrite Perovskite Electrodes of Solid Oxide Fuel Cells – a Review. International Journal of Hydrogen Energy 2019 , 44 (14), 7448–7493. DOI:10.1016/j.ijhydene.2019.01.212. Hussain, S.; Yangping, L. Review of Solid Oxide Fuel Cell Materials: Cathode, Anode, and Electrolyte. Energy Transitions 2020 , 4 (2), 113–126. DOI:10.1007/s41825-020-00029-8. Zhang, S.; Wan, Y.; Xu, Z.; Xue, S.; Zhang, L.; Zhang, B.; Xia, C. Bismuth Doped La 75 Sr 0.25 Cr 0.5 Mn 0.5 O 3−δ Perovskite as a Novel Redox-Stable Efficient Anode for Solid Oxide Fuel Cells. Journal of Materials Chemistry A 2020 , 8 (23), 11553–11563. DOI:10.1039/d0ta03328f. de Larramendi, I. R.; Ortiz-Vitoriano, N.; Dzul-Bautista, I. B.; Rojo, T. Designing Perovskite Oxides for Solid Oxide Fuel Cells. Perovskite Materials - Synthesis, Characterisation, Properties, and Applications 2016 . DOI:10.5772/61304. Ansari, H. M.; Addo, P. K.; Mulmi, S.; Yuan, H.; Botton, G. A.; Thangadurai, V.; Birss, V. I. Deciphering the Interaction of Single-Phase La 3 Sr 0.7 Fe 0.7 Cr 0.3 O 3-δ with CO2/CO Environments for Application in Reversible Solid Oxide Cells. ACS Applied Materials & Interfaces 2022 , 14 (11), 13388–13399. DOI:10.1021/acsami.2c00857. Addo, P. K.; Molero-Sanchez, B.; Buyukaksoy, A.; Paulson, S.; Birss, V. Sulfur Tolerance of La 3 M 0.7 Fe 0.7 Cr 0.3 O 3-δ (M= Sr, Ca) Solid Oxide Fuel Cell Anodes. ECS Transactions 2015 , 66 (2), 219–228. DOI:10.1149/06602.0219ecst. Molero-Sánchez, B.; Prado-Gonjal, J.; Ávila-Brande, D.; Chen, M.; Morán, E.; Birss, V. High Performance La 3 Ca 0.7 Cr 0.3 Fe 0.7 O 3−δ Air Electrode for Reversible Solid Oxide Fuel Cell Applications. International Journal of Hydrogen Energy 2015 , 40 (4), 1902–1910. DOI:10.1016/j.ijhydene.2014.11.127. Molero-Sánchez, B.; Addo, P.; Buyukaksoy, A.; Birss, V. Performance Enhancement of La 3 Ca 0.7 Fe 0.7 Cr 0.3 O 3-δ Air Electrodes by Infiltration Methods. Journal of The Electrochemical Society 2017 , 164 (10). DOI:10.1149/2.0151710jes. Ansari, H. M.; Bass, A. S.; Ahmad, N.; Birss, V. I. Unraveling the Evolution of Exsolved Fe–Ni Alloy Nanoparticles in Ni-Doped La 3 Ca 0.7 Fe 0.7 Cr 0.3 O
3−
δ
and Their Role in Enhancing CO 2 –CO Electrocatalysis. Journal of Materials Chemistry A 2022 , 10 (5), 2280–2294. DOI: 10.1039/D1TA07552G Zhang, W.; Hu, Y. H. Material Design and Performance of Carbon Monoxide‐fueled Solid Oxide Fuel Cells: A Review. Energy Science & Engineering 2023 , 11 (9), 3276–3288. DOI:10.1002/ese3.1502. Figure 1 Figure 2