Understanding the dissolution of silicate glasses and minerals from atomic to macroscopic levels is a challenge with major implications in geoscience and industry. One of the main uncertainties limiting the development of predictive models lies in the formation of an amorphous surface layer––called gel––that can in some circumstances control the reactivity of the buried interface. Here, we report experimental and simulation results deciphering the mechanisms by which the gel becomes passivating. The study conducted on a six-oxide borosilicate glass shows that gel reorganization involving high exchange rate of oxygen and low exchange rate of silicon is the key mechanism accounting for extremely low apparent water diffusivity (∼10−21 m2 s−1), which could be rate-limiting for the overall reaction. These findings could be used to improve kinetic models, and inspire the development of new molecular sieve materials with tailored properties as well as highly durable glass for application in extreme environments.
Knowing the structure of a material is necessary to understand its evolution under various influences; here, the alteration by water of a reference glass of nuclear interest, called International Simple Glass (ISG), is studied. The ISG atomic structure has not yet been thoroughly characterized. Short- and medium-range order in this six-oxide glass was investigated by molecular dynamics (MD) methods. Combining the simulated data with experimental observations acquired from both pristine and altered ISG provided new insight into the formation of surface layers and passivation of the underlying glass. In the tested conditions of 90 °C, silica-saturated solution, and pH90°C 7, the passivating layer partly inherits the structure of the pristine glass network despite the release of mobile elements (Na, B, and some Ca), with a reorganization of the silicate network following B release. The layer appears to minimize its internal energy by relaxing strain accumulated during glass quenching. The resulting passivated glass shows a strong resistance to hydrolysis. The nanopores of this hydrated material, displaying a mean pore size of ∼1 nm, are filled with various water species. Water speciation determination inside the nanopores is therefore an achievement for future water dynamic study in the passivated glass.
The porosity and pore-size distribution in the glass play an important role in glass corrosion; however, such information is difficult to be obtained non-destructively. Here we report the use of spectroscopic ellipsometry (SE) under controlled humidity environments to determine those structural parameters in the alteration layers formed on international simple glass (ISG), a model nuclear waste glass, in aqueous corrosion conditions. The SE results show that the ISG sample corroded for nearly 4.5 years develops pores larger than 2 nm in diameter, while the alteration layers formed initially in less than 1 month do not have such large pores. The development of larger pores over a long period of corrosion time, while the overall thickness remains relatively constant, implies structural rearrangements of the silicate network occurring within the alteration layer, which could eventually affect the transport of reactants and products as well as the structural stability.
Amorphous silica-rich surface layers, also called gels, can passivate silicate glass and minerals depending on environmental conditions. However, several uncertainties remain on the mechanisms controlling the formation of these layers. In this paper, the influence of exogenous ions supplied by solutions is studied, both on the formation and on the properties of the gel formed on international simple glass (ISG). ISG was altered at 90 °C, pH90°C 7, in silica-saturated solutions containing various alkaline cations separately (Li+, Na+, K+, and Cs+). The alteration kinetics observed with Li and Na in the solution is similar to that observed with no ions, while K and Cs in the solution tend to decrease glass alteration. Furthermore, for K or Cs ions, the kinetics decreases as the ionic strength of the solution increases. The passivation layer formed in these solutions shows a selectivity toward cations following the series K > Cs > Na >> Li. These alkalis replace Ca from pristine glass in the altered structures, leading to differences in [AlO4]− units charge compensation. Importantly, exchange between Ca and alkali also affects the total quantity of water inside each gel and this effect is well correlated with the observed drop in glass alteration.