1 December 2010 in Journal of Applied Physics
Vanadium dioxide exhibits a well-known insulator-to-metal transition during which several of its physical properties change significantly. A hysteresis loop develops for each of them as the material is heated and then cooled through the transition. In this work samples were maintained—by heat sinking—at a selected temperature within the heating branch of the hysteresis loops for resistance and near-infrared transmittance, while brief thermal excursions of the film were caused by either voltage pulses applied to the film or laser light pulses irradiating the film. These pulses had durations from milliseconds to a few seconds and the resulting drops in resistance or transmittance were easily and repeatably measurable without appreciably affecting their new values. A sequence of equal-duration pulses (for either equal-voltage or equal-irradiation pulses) caused the resistance and infrared transmittance to continue to drop, each time by a smaller amount, and larger energy pulses were required in order to cause drops comparable with the initial one. The ability of the film to change the values of the measurands in this manner with additional pulses was maintained up to a limit defined by the outer hysteresis curve for the measurand in question. The results presented show that a plurality of memory “states” in can be established or “written” either by voltage pulses or by light pulses applied to the material, and queried or “read” by resistance or transmittance readings, or both. These states were found to remain stable for at least several hours, as long as temperature was kept constant, and are expected to persist indefinitely under this condition. In the all-optical case, if the same light beam is used for writing and reading the memory state, the device is an optical analog of a memristor.
15 May 2012 in Journal of Applied Physics
Silicon microcantilevers were coated by pulsed laser deposition with vanadium dioxide (VO2) (monoclinic M1 phase) and V1−xCrxO2 with x near 0.024 (monoclinic M2 phase), and their mechanical characteristics were studied as a function of temperature through the films’ insulator-to-metal transition (IMT). The undoped VO2 films grew with (011)M1 planes parallel to the substrate, while Cr-doped VO2 films grew oriented with (201)M2 and ( )M2 planes parallel to the substrate. In both cases, the films transformed reversibly through the IMT to the tetragonal (rutile, R) phase, with film (110)R planes oriented parallel to the substrate. The fundamental resonant frequencies of the cantilevers were measured as the temperature was cycled from ambient temperature, through the IMT, and up to 100 °C. Very high resonant frequency changes were observed through the transition for both types of samples, with increases during heating of over 11% and over 15% for the cantilevers coated with pure and Cr-doped VO2, respectively. From the resonant frequencies measured at room temperature for the bare and coated cantilevers in each case, the effective Young’s moduli of the films were determined. The values obtained, assuming bulk densities for the films, are 156 ± 7.5 GPa for VO2 (M1 phase) and 102 ± 3 GPa for Cr-doped VO2 (M2 phase). Strong curvature changes during the transition to the R phase were also observed for cantilevers coated with both types of films, but these were significantly higher in the case for the Cr-doped film. Curvature changes for temperature ranges outside the IMT region were small and attributed to differential thermal expansion between film and silicon substrate. From measured cantilever tip displacements in this post-transition range—for the undoped VO2-coated microcantilevers—a rough estimate of 110 GPa was obtained for the effective Young’s modulus for R-phase VO2. The substantially higher changes in resonant frequency and curvature for V1−xCrxO2-coated cantilevers suggest that this material may be even more useful than M1-phase VO2 for prospective microelectromechanical or optomechanical device applications in which ample frequency tunability—in oscillators or filters—or large displacements—in actuators—within a small temperature range is desirable. Since M2-phase V1−xCrxO2 with Cr composition of a few atomic percent retains other desirable properties of VO2, such as very high resistivity changes through the IMT and a transition temperature fairly close to ambient temperature, multifunctionality is not impaired and in fact may be enhanced for some applications.
12 May 2008 in Applied Physics Letters
Young’s modulus of thin films has been measured for the first time through the material’s insulator-to-metal transition. The resonant frequency of silicon coated cantilevers was measured in the temperature range . It has been found that during the semiconductor to metallic transition of thin films, which occurs at a temperature of , Young’s modulus changes most dramatically with temperature, abruptly reversing its declining trend with increasing temperature. The film is stiffened through the transition and, as the temperature is further raised, the declining trend is reasserted at a similar rate.
1 November 2011 in Journal of Applied Physics
The dynamic response of VO2-coated silicon microcantilevers thermally driven over the film’s insulator-to-metal transition was studied using laser light pulses directly incident on the cantilevers. The measured photothermal response revealed very high curvature changes of approximately 2500 m−1 up to pulse frequencies greater than 100 Hz and readily observable vibrations up to frequencies of a few kHz with no amplitude degradation after tens of thousands of pulses. Maximum tip amplitudes for 300-μm-long, 1-μm-thick cantilevers used in these experiments were nearly 120 μm and correspondingly less for 2-μm-thick cantilevers. The main mechanism limiting oscillation amplitude was found to be heat transport response during heating and cooling, which depends mainly on thermal conduction through the cantilever itself to the massive anchor and chip body, which acted as a heat sink at room temperature. For the laser-driven oscillations studied, damping by the surrounding air is unimportant in the range of frequencies probed. Large-curvature response is expected to extend to higher pulse frequencies for cantilevers with smaller dimensions.
3 August 2012 in Smart Materials and Structures
14 September 2013 in Physica Status Solidi (a)
The structural phase transition in vanadium dioxide and its inherent hysteretic behavior are used in the work by Cabrera et al. (pp. 1704–1711) to program multiple mechanical states in a micrometer-sized structure through electrical pulses. The background image on the cover shows one of the lithography masks used for the fabrication of the device. In the top-left 3D scheme of the micro-actuator a two-end arrow at the tip emphasizes the fact that bi-directional mechanical states were programmed. The gray part of the actuator represents the metal traces used for Joule heating, and the cantilever made of SiO2 (glass) is shown as transparent. The bottom plots are a graphical representation of the mechanical states (deflection) that can be programmed with the electrical pulses (voltage). Two horizontal rectangles in the deflection graph represent the windows for programming an “on-state” and an “off-state”. Finally, the monoclinic and tetragonal lattice diagrams emphasize that the phenomena that allow for the mechanical states to be programmed are the crystallographic changes in the VO2 thin film that occur across the phase transition and are completely reversible.