Owing to the insufficient converter heat, IF steel is produced via the BOF–LF–RH–CC process in Pangang Group Xichang Steel and Vanadium Co., Ltd. To clarify the evolution of inclusions and the control strategy to improve the cleanliness of molten steel in Ti-bearing IF steel produced via the long process, scanning electron microscopy with energy spectroscopy analysis and automatic scanning electron microscopy were employed to analyze the number, size, type and morphology of inclusions in IF steel from RH to tundish. The results show that the characteristics of inclusions are similar in two heats during RH treatment. In the tundish sample of Heat 2, the number density (ND) and area fraction (AF) of Al2O3 and Al2O3·TiOx inclusions increase significantly, and the size of Al2O3 inclusions decreases obviously, which is closely related to the serious reoxidation of molten steel caused by the slag with high oxidability during the holding process. Meanwhile, a new method of determining the number of cluster inclusions is used to evaluate the cleanliness of IF steel in this paper, and the obtained number of inclusion clusters is consistent with the trend of ND and AF of inclusions. The effects of reoxidation on the morphology, number and other indexes of Al2O3 and Al2O3·TiOx inclusions are discussed in detail, and there are two ways of forming Al2O3·TiOx inclusions in the case of serious reoxidation. To weaken the reoxidation process and enhance the cleanliness of IF steel produced via the long process, reducing the oxygen content in molten steel before Al deoxidation, minimizing the holding time and reducing the oxidability of slag after RH are helpful.
28 July 2022 in Metallurgical Research & Technology
A new mathematical model for the RH forced oxygen blowing decarburization process which takes the influence of post combustion on decarburization into account is established. Decarburization reactions are considered to take place at four reaction sites. The simulated results of carbon and oxygen contents show relatively good agreement with the experimental data under different oxygen flow rates. At the rapid decarburization stage including the O2 blowing process, 66.1% of the total decarburization amount is removed. By using the forced oxygen blowing decarburization process, the decarburization rate in the bulk steel is improved most significantly. Additionally, the effects of oxygen flow rates on carbon, oxygen and total decarburization rate are evaluated in detail. At 1500 m3 · h−1, the oxygen content is adequate to completely remove carbon of molten steel in the vacuum vessel during the O2 blowing. Combining with the analysis of oxygen flow rates on the decarburization rate at each site, 1500 m3 · h−1 is chosen as the critical oxygen flow rate to achieve the best decarburization performance. The influences of other parameters including initial carbon and oxygen contents and oxygen utilization rate on decarburization are also investigated.
22 July 2024 in Ironmaking & Steelmaking: Processes, Products and Applications
The effect of slag composition on the cleanliness of Al-Ti deoxidized interstitial-free steel produced via basic oxygen furnace (BOF)-ladle furnace (LF)-Ruhrstahl-Heraeus (RH)-continuous casting (CC) process was investigated by the systematic samplings and analyses for four heats in a steel plant in China. Oxygen/nitrogen analyzer, automatic scanning electron microscope, field-emission scanning electron microscope, and energy spectroscopy analysis were used to analyze the variations of number, size, type, and morphology of inclusions in molten steel from RH to tundish, and X-ray fluorescence was used to analyze the slag composition. The relationship between slag composition and inclusion characteristics in molten steel was investigated. The effect of slag composition on the oxygen mass transfer from the slag–metal interface to liquid steel was also studied through a theoretical calculation. The results showed that the cleanliness of molten steel was greatly affected by the slag composition. The deterioration of steel cleanliness was mainly arisen from a serious reoxidation of molten steel by oxidizing components like (T.Fe + MnO) in top slag during RH refining process. A weak ability to absorb inclusions of top slag with high CaO/Al2O3 and CaO/SiO2 mass ratios was confirmed from the inclusions analyses. The size and number of Al2O3 inclusion clusters were larger, and Ti content in Al2O3-TiO x inclusions was higher from RH to tundish in the case of serious reoxidation. The reduction of FeO content and keeping the CaO/Al2O3 and CaO/SiO2 ratios at about 1.6 and 4–7, respectively, in top slag during RH refining process was beneficial to minimize the reoxidation of Al and Ti and increase the inclusion absorption ability of top slag.
The novel industrial trial is conducted to investigate the effect of argon injection into the down-leg of the RH degasser on the inclusion removal. The ‘cold steel plate dipping’ is used to take samples of molten steel and argon bubbles from the RH ladle. The industrial CT detection and electron microscope observation are applied to analyze the bubble characteristics. The results show that the size of bubbles generated by argon injection in the down-leg ranges from 7 to 1430 μm. Among them, the number density of bubbles with a diameter of 60 μm is the largest, reaching 0.1 per mm3. After adopting the down-leg argon injection technology, the average oxygen activity at the end of the RH process decreases by 2.35 ppm, and the surface defects of cold-rolled sheets of all grades are reduced. Based on the theoretical analysis of bubble collision and adhesion to inclusions, the small-sized bubbles have a relatively high capture probability for inclusions smaller than 10 μm. Comprehensively analyzing the experimental results, it is found that the down-leg argon injection technology has an obvious effect on removing inclusions.
Macrosegregation in continuous casting slabs remains a critical defect that adversely affects the homogeneity and mechanical properties of the final rolled products. Industrial experiments were conducted on E355 steel continuous casting slabs to investigate the effects of electromagnetic stirring (EMS) and soft reduction (SR) on the evolution of slab macrosegregation. Furthermore, the inheritance of segregation from the slab to the rolled plate was analyzed. The results indicate that the equiaxed crystal ratio increases and the centerline segregation decreases with increasing stirring intensity. The application of both secondary EMS and SR minimized the centerline segregation in the slab. When the current intensity was increased from 0 A to 320 A in continuous stirring mode, the equiaxed crystal fraction increased from 22.52% to 32.52%, and the centerline segregation index decreased from 1.23 to 1.17. Compared with the continuous stirring mode, the alternating stirring mode promoted a more pronounced increase in the equiaxed crystal ratio and a further reduction in the centerline segregation. The centerline segregation in the slab correlates with the banded structure observed in the rolled plate. A higher degree of slab centerline segregation corresponds to a more severe banded structure and greater fluctuations in the mechanical properties of the plate. Through parameter optimization, the recommended settings are an alternating stirring mode with a current of 320 A at 5 Hz and an SR amount of 3 mm. Under these optimized conditions, the equiaxed crystal ratio of the slab increased to 35.22%, the centerline segregation index dropped to 1.15, and the banded structure in the rolled plate was reduced to grade 2.0. Consequently, the standard deviations of the tensile strength and elongation were 8.03 MPa and 1.1%, respectively.
23 March 2026 in Ironmaking & Steelmaking: Processes, Products and Applications
For the submerged entry nozzle (SEN) samples obtained during continuous casting of Ti-IF steels with different Ti contents, the characteristics of the SEN deposits were systematically studied using X-ray fluorescence, X-ray diffraction, and scanning electron microscope with energy-dispersive spectroscopy (SEM-EDS). The cleanliness of various Ti-IF steel slabs was analyzed using automatic scanning microscope, SEM-EDS, and oxygen/nitrogen analyzer. The experimental results show that the nozzle deposits for the Ti-IF steel with high Ti content can be divided into three layers. However, for the Ti-IF steel with low Ti content, it consists only of two layers. As the Ti content in the Ti-IF steel increases, the Ti element in the nozzle deposits aggregating significantly, and the cleanliness of Ti-IF steel slabs worsens gradually, and the possibility and severity of the nozzle clogging also increase accordingly. Therefore, two different clogging mechanisms for Ti-IF steels with various Ti contents were obtained in this paper.