To investigate the relationship between surface microstructure and wear mechanism in D2/U71Mn wheel-rail material under different contact stress conditions, rolling wear tests using a GPM-40 wear machine to simulate the wheel-rail operation was performed. After wear tests, an optical microscope (OM), scanning electron microscope (SEM) and micro-hardness testers were used to characterize the microstructure and fatigue wear cracks. The results show that the thickness of the plastic deformation layer and surface hardness is increased with the increase of contact stress. Under high contact stress condition (1200 MPa), the severe plastic deformation layer led to the formation of fatigue wear of wheel-rail samples. Under a contact stress of 700 MPa, the wear mechanism of samples is adhesive wear and wear rate is low. With the increase of contact stress, the fatigue cracks are gradually severe. Under a contact stress of 1200 MPa, the wear mechanism of samples becomes fatigue wear and the fatigue wear cracks cause the increase of wear rate. The fatigue wear can accelerate the wear failure of wheel-rail samples. The fatigue wear cracks of wheel samples are severer than that of rail samples due to both the rate of plastic strain and the content of proeutectoid ferrite.
In this paper, the influence of a surface ultrasonic rolling process on the surface integrity of TC4 titanium alloy and its influence on the fatigue properties were studied. By comparing and analyzing the surface roughness, microhardness, residual stress, microstructure, and fatigue fracture, the surface strengthening and modification mechanism of TC4 titanium alloy is discussed. The results show that the surface roughness of titanium alloy is observably decreased after the suitable surface ultrasonic rolling process, and the maximum Ra value can be reduced to 0.052 μm. The axial residual stress on the specimen surface can be increased to −685 MPa. The hardening rate of the surface hardness of the sample was 35%. The residual compressive stress and hardness of the sample surface increased with the increase of static pressure. However, the increase of feed rate and rational speed was less. After surface ultrasonic rolling, the sample surface exhibited obvious grain refinement, the number of high-angle boundaries increased to include the formation of nano-equiaxed grains. The fatigue strength increased by 52% from 280 MPa to 425 MPa. Under 450 MPa, the fatigue life of samples with SUR 2 was the highest, at about 7.7 times that of the original samples. The surface integrity of titanium alloy samples after surface ultrasonic rolling treatment is greatly improved, which is the reason for the significant increase in fatigue life of the samples.
A GPM-30 fatigue machine was used to investigate the influence of surface ultrasonic rolling (SURT) on the rolling contact fatigue (RCF) life of D2 wheel steel. The experimental results present that the RCF life of the grinding processing sample is 4.1 × 105 cycles. During the RCF process, the flaking of the fine grain layer and high surface roughness of the grinding processing sample cause the production of RCF cracks. When the samples are treated by SURT with 0.2 MPa and 0.4 MPa, the RCF life is 9.2 × 105 cycles and 9.6 × 105 cycles, respectively. After SURT, the surface roughness of the samples is reduced, and a certain thickness of gradient-plastic-deformation layer and a residual-compressive-stress layer are produced. These factors lead to the improvement of the RCF property. However, when the static pressure increases to 0.6 MPa during SURT, the RCF life of the sample is reduced during RCF testing. The micro-cracks, which are formed during SURT, become the crack source and cause the formation of RCF cracks, decreasing of the RCF life.
In this paper, the effect of surface ultrasonic rolling treatment (SURT) on surface properties of T4003 cold metal transfer (CMT) welded joints was studied. Surface topography and microstructure changes of the welded joint surface before and after SURT were observed by optical microscope and scanning electron microscope. The hardness and residual stress distribution of welded joint were measured by a microhardness tester and X-ray diffractometer. The change of corrosion resistance of welded joints was studied by electrochemical polarization curve measurement. The results show that surface roughness (Ra) of the weld zone, heat affect zone (HAZ), and base metal after SURT was reduced to 0.320 μm, 0.156 μm, and 0.227 μm, respectively, and surface morphology became smooth. The plastic deformation layer and working hardening layer were formed at the welded joint. The degree of plastic deformation of the weld zone was more serious than that in the base metal, and grains in weld zone was obviously refined. The thickness of plastic deformation layer was about 100 μm. The surface hardness in the weld zone was highest, which is about 420 HV. The refinement of grains and the increase of surface hardness can improve the fatigue life of welded joint. After SURT, the residual stress in the welded joint changes from residual tensile stress to residual compressive stress, which can also improve fatigue life of the welded joint. Surface corrosion resistance of welded joints after SURT was improved due to smooth surface and the formation of fine grains layer.