This study focuses on the characterization of the failure behavior of an extruded Mg10Dy1Nd alloy during stress corrosion. The microstructure, hardness, strength and corrosion behavior of binary alloys Mg10Dy and Mg1Nd are compared to those of the ternary alloy system. The ternary alloy Mg-Dy-Nd that is not fully recrystallized has the highest hardness but lacks ductility. The investigated alloys twin during plastic deformation. Static C-ring tests in Ringer solution were used to evaluate the stress corrosion properties, and stress corrosion could not be found. None of the alloys failed by fracturing, but corrosion pits formed to various extents. These corrosion pits were elliptical in shape and located below the surface. Some of the pits reduced the remaining wall thickness significantly, but the stress increased by the notch effect did not lead to crack initiation. Furthermore, the C-ring specimen was subjected to compressive loading until fracture. Whereas the Mg1Nd alloy showed ductile behavior, the alloys containing Dy fractured on the tensile side. The crack initiation and growth were mainly influenced by the twin boundaries. The Mg10Dy1Nd alloy had an inhomogeneous microstructure and low ductility, which resulted in a lower fracture toughness than that of the Mg10Dy alloy. There were features that indicate hydrogen-assisted fracture. Although adding Nd decreased the fracture toughness, it reduced the grain size and had a positive influence on the corrosion rate during immersion testing.
The objective of this study is the investigation of nanomechanical properties using nanoindentation of extruded and heat-treated Mg-Dy-Nd-Zn-Zr, with an emphasis on the transformation of long-period stacking-ordered (LPSO) phases. Solution heat treatment was performed with different heat treatment for durations on hot extruded Mg-Dy-Nd-Zn-Zr to monitor the transformation of LPSO phases, as well as to keep track of microstructural changes. The initial fine-grained microstructure, with blocky and lamellar LPSO structures within the matrix, first transformed into coarser grains with fewer LPSO lamellae, which then increased in amount again at higher annealing duration. The blocky LPSO phases, which have the highest hardness compared to the matrix grains with and without LPSO lamellae, consistently decrease in quantity, as so does the trend in their hardness value. The Mg matrix grains with LPSO lamellae show a lower hardness compared to the Mg matrix grains without or with a just few lamellar LPSO phases, and increase in quantity at long annealing durations. The overall hardness of the microstructure is essentially determined by the LPSO lamellae-containing grains and reaches a peak at 24 h. There is another peak found for the grain size values; however, this is at later annealing duration, at 72 h. The reduction in grain size towards longer annealing durations goes along with a reactivated formation of LPSO lamellae.
The investigation of the crack propagation in as-extruded and heat-treated Mg-Dy-Nd-Zn-Zr alloy with a focus on the interaction of long-period stacking-ordered (LPSO) structures is the aim of this study. Solution heat treatment on a hot extruded Mg-Dy-Nd-Zn-Zr (RESOLOY®) was done to change the initial fine-grained microstructure, consisting of grain boundary blocky LPSO and lamellar LPSO structures within the matrix, into coarser grains of less lamellar and blocky LPSO phases. C-ring compression tests in Ringer solution were used to cause a fracture. Crack initiation and propagation is influenced by twin boundaries and LPSO lamellae. The blocky LPSO phases also clearly hinder crack growth, by increasing the energy to pass either through the phase or along its interface. The microstructural features were characterized by micro- and nanohardness as well as the amount and location of LPSO phases in dependence on the heat treatment condition. By applying nanoindentation, blocky LPSO phases show a higher hardness than the grains with or without lamellar LPSO phases and their hardness decreases with heat treatment time. On the other hand, the matrix increases in hardness by solid solution strengthening. The microstructure consisting of a good balance of grain size, matrix and blocky LPSO phases and twins shows the highest fracture energy.
Flow diverter devices are small stents used to divert blood flow away from aneurysms in the brain, stagnating flow and inducing intra-aneurysmal thrombosis which in time will prevent aneurysm rupture. Current devices are formed from thin (∼25 μm) wires which will remain in place long after the aneurysm has been mitigated. As their continued presence could lead to secondary complications, an absorbable flow diverter which dissolves into the body after aneurysm occlusion is desirable. The absorbable metals investigated to date struggle to achieve the necessary combination of strength, elasticity, corrosion rate, fragmentation resistance, radiopacity, and biocompatibility. This work proposes and investigates a new composite wire concept combining absorbable iron alloy (FeMnN) shells with one or more pure molybdenum (Mo) cores. Various wire configurations are produced and drawn to 25-250 μm wires. Tensile testing revealed high and tunable mechanical properties on par with existing flow diverter materials. In vitro degradation testing of 100 μm wire in DMEM to 7 days indicated progressive corrosion and cracking of the FeMnN shell but not of the Mo, confirming the cathodic protection of the Mo by the FeMnN and thus mitigation of premature fragmentation risk. In vivo implantation and subsequent μCT of the same wires in mouse aortas to 6 months showed meaningful corrosion had begun in the FeMnN shell but not yet in the Mo filament cores. In total, these results indicate that these composites may offer an ideal combination of properties for absorbable flow diverters.
DieMag633, a cast Mg-Al-Ba-Ca alloy, was the focus of this study. Brittle interdendritic phases strongly influenced the crack initiation and propagation under quasi-static and fatigue loading. Especially under tensile loading, the material showed a low resistance to failure. Selected fatigue loading sequences were applied to investigate their influence on crack propagation. DieMag633 in this study contained shrinkage cavities and pores of significant size and irregular distribution. Even though pores played a role in initiating the crack, it was mainly influenced by the Ba- and Ca-rich phases, being and staying much harder under deformation than the Mg-matrix. Apart from the fatigue crack propagation region under fatigue loading, there was no transgranular cracking found within the dendritic α-Mg grains. Only under compression did the dendritic α-Mg grains bridge the crack from one brittle phase to another. Transgranular cracking within the compact Ba-rich phase was very pronounced, starting with many microcracks within this phase and then connecting to the macrocrack. The lamellar Ca-rich phase showed also mainly transgranular cracking, but being small lamellae, intergranular cracking was additionally found. The hardness increase under deformation depended on the loading condition; a compression load strain-hardened the material the most. µCT analysis was applied to characterize the amount and location of the shrinkage cavities and pores in the individual gauge length.
Flanging is a widespread method in the sheet metal working industry to connect same or different materials by forming. Especially the sealing technology makes high demands on the flanging process: a low sheet thickness of the inner eyelet is necessary for proper sealing. The outer edges of the neck rings are mostly manufactured by shear cutting. The quality of the cut surface and the level of the local strain hardening influence decisively the limit of the flanging process by possible cracking. This paper is focused on the dependencies of these factors regarding thin metal sheets of different materials with a thickness down to 100 μm. It could be shown that strain hardening has a stronger effect on the process limits compared to the notch effect of the sheet edges when using standard values for the clearance of the shear cutting tool. Furthermore, a process is investigated with a partial inductive short-time heat treatment of the most deformed edge area. Due to the low thickness of the material and low heat capacities related thereto, it is possible to integrate a recrystallization annealing as single step into the forming process. As a result, the strain hardening can be removed from the affected zone directly between two forming steps to increase the process limits.