With the development of 3D printing technology, there is a need to produce printable materials with improved properties, e.g., sliding properties. In this paper, the authors present the possibilities of producing composites based on biodegradable PLA with the addition of graphite. The team created composites with the following graphite weight contents: 1%, 2.5%, 5%, 7.5%, and 10%. Neat material was also subjected to testing. Tribological, mechanical, and chemical properties of the mentioned materials were examined. Measurements were also made after keeping the samples in ageing and climatic ovens. Furthermore, SEM observations of samples before and after friction tests were carried out. It was demonstrated that increasing graphite content caused a significant decrease in wear (PLA + 10% graphite had a wear rate three times lower than for a neat material). The addition of graphite did not adversely affect most of the other properties, but it ought to be noted that mechanical properties changed significantly. After conditioning in a climatic oven PLA + 10% graphite has (in comparison with neat material) 11% lower fracture stress, 47% lower impact strength, and 21% higher Young’s modulus. It can be certainly stated that the addition of graphite to PLA is a step towards obtaining a material that is low-cost and suitable for printing sliding spare parts.
MoS2 is an additive used to improve the tribological properties of plastics. In this work, it was decided to verify the use of MoS2 as a modifier of the properties of PLA filaments used in the additive FDM/FFF technique. For this purpose, MoS2 was introduced into the PLA matrix at concentrations of 0.025–1.0% by weight. Through extrusion, a fibre with a diameter of 1.75 mm was obtained. 3D printed samples with three different filling patterns were subjected to comprehensive thermal (TG, DSC and HDT), mechanical (impact, bending and strength tests), tribological and physicochemical characteristics. The mechanical properties were determined for two different types of fillings, and samples with the third type of filling were used for tribological tests. Tensile strength has been significantly increased for all samples with longitudinal filling with improvement up to 49%. In terms of tribological properties, higher values of the addition (0.5%) caused a significant increase of up to 457% of the wear indicator. A significant improvement in processing properties in terms of rheology was obtained (416% compared to pure PLA with the addition of 1.0%), which translated into more efficient processing, increased interlayer adhesion and mechanical strength. As a result, the quality of printed objects has been improved. Microscopic analysis was also carried out, which confirmed the good dispersion of the modifier in the polymer matrix (SEM-EDS). Microscopic techniques (MO, SEM) allowed for the characterization of the effect of the additive on changes in the printing process (improvement of interlayer remelting) and to assess impact fractures. In the tribological area, the introduced modification did not bring spectacular effects.
Plastics are widely used due to their numerous advantages. Unfortunately, most of their types do not decomposequickly in the natural environment, causing environmental pollution. In order to counteract the problem ofwaste, there is a growing interest in plastics that degrade under the influence of the natural environment.The authors of this article are trying to use biodegradable plastic for sliding elements. Polylactide (PLA)is a biodegradable, environmentally friendly polymer; however, it has a high wear and friction coefficientwhen working with steel. It was decided to check whether the addition of 10% graphite (a commonly used,environmentally friendly modifier) would improve the tribological properties of PLA. Using a pin-on-discstation, the coefficient of friction, wear and temperature of the sample were determined depending on thespeed of cooperation and pressure. The addition of graphite significantly reduced the linear wear of thecomposite in a wide range of parameters (sliding speed and pressure), slightly decreased the coefficient offriction and slightly increased the temperature of the composite.
Przedmiotem analizy są strunobetonowe dźwigarydachowe systemu P70 (SBn-I-65/15). Produkowano je w wersjiumożliwiającej wzmocnienie nadbetonem ułożonym międzyprefabrykowanymi płytami dachowymi, dzięki czemu uzyskiwanopełną projektowaną nośność. W trakcie oględzin analizowanegoobiektu stwierdzono, iż nadbeton taki wykonano, jednaknie w obrębie świetlików kalenicowych, gdzie wykonano wyłącznienadbeton spadkowy. Z tego względu odcinek pod świetlikamijest krytyczny z punktu widzenia bezpieczeństwa konstrukcji.Brak nadbetonu jest również powodem znaczących ugięć dźwigarów.W pracy przedstawiono wyniki oceny stanu technicznego,badań, pomiarów geodezyjnych ugięć i sprawdzających obliczeństatyczno-wytrzymałościowych oraz sposób wzmocnienia dźwigarów,umożliwiający jego realizację na czynnym obiekcie