Iron nanopowder could be used as a sintering aid to water-atomised steel powder to improve the sintered density of metallurgical (PM) compacts. For the sintering process to be efficient, the inevitable surface oxide on the nanopowder must be reduced at least in part to facilitate its sintering aid effect. While appreciable research has been conducted in the domain of oxide reduction of the normal ferrous powder, the same cannot be said about the nanometric counterpart. The reaction kinetics for the reduction of surface oxide of iron nanopowder in hydrogen was therefore investigated using nonisothermal thermogravimetric (TG) measurements. The activation energy values were determined from the TG data using both isoconversional Kissinger–Akahira–Sunose (KAS) method and the Kissinger approach. The values obtained were well within the range of reported data. The reaction kinetics of Fe2O3 as a reference material was also depicted and the reduction of this oxide proceeds in two sequential stages. The first stage corresponds to the reduction of Fe2O3 to Fe3O4, while the second stage corresponds to a complete reduction of oxide to metallic Fe. The activation energy variation over the reduction process was observed and a model was proposed to understand the reduction of surface iron oxide of iron nanopowder.
1 July 2020 in Metallurgical and Materials Transactions A
A promising method of improving the densification of powder metallurgical steel components is to blend nanopowder with the otherwise typically used micrometre-sized powder. The higher surface-to-volume ratio of nanopowder is hypothesized to accelerate the sintering process and increase the inter-particle contact area between the powder particles. This is supposed to enhance the material transport and improve the densification. In the present investigation, water-atomized iron powder (− 45 μm) was mixed separately with pure iron and low-carbon steel nanopowder, each at a ratio of 95 to 5 pct. These powder mixes were compacted at different pressures (400, 600 and 800 MPa) and then sintered at 1350 °C in a pure hydrogen atmosphere. The sintering behavior of the powder blend compacts was compared to that of the compact with micrometre-sized powder only. Densification commenced at much lower temperatures in the presence of nanopowder. To understand this, sintering at intermittent temperatures such as 500 °C and 700 °C was conducted. The fracture surface revealed that the nanopowder was sintered at between 500 °C and 700 °C, which in turn contributed to the densification of the powder mix at the lower temperature range. Based on the sintering experiments, an attempt was made to calculate the activation energy and identify the associated sinter mechanism using two different approaches. It was shown that the first approach yielded values in agreement with the grain-boundary diffusion mechanism. As the nanopowder content increased, there was an increase in linear shrinkage during sintering.
Internal combustion engine downsizing and powertrain electrification trends in recent years have led to higher thermal loads on the cylinder head materials with an increased number of engine start–stop thermal load cycles. This requires designing cylinder heads that are resilient against thermomechanical fatigue damage. To reduce the developmental costs, reliable numerical models for use in computer-aided design approaches are required. Thus, a comprehensive understanding of the material deformation behaviour under loads mimicking in-service conditions is desired to make better engineering decisions. This study examines the effect of strain rate on the cyclic deformation behaviour of the A356-T7 + 0.5% Cu aluminium alloy commonly used in modern internal combustion engine cylinder heads. Samples extracted from the valve bridge areas of the cylinder heads are tested in strain-controlled fatigue tests. Samples are tested at strain rates of 1% s−1 and 10% s−1 at room temperature, 150 and 200 °C. The material exhibits increased isotropic hardening and softening rates and an increased number of cycles to failure at 10% s−1. The strain rate has a dramatic influence on the mean stress development at room temperature. The role of silicon particles in the fracture mechanism is investigated using electron microscopy techniques.
Water‐atomized iron and steel powder is commonly used as the base material for powder metallurgy (PM) of ferrous components. The powder surface chemistry is characterized by a thin surface oxide layer and more thermodynamically stable oxide particulates whose extent, distribution, and composition change during the sintering cycle due to a complex set of oxidation–reduction reactions. In this study, the surface chemistry of iron and steel powder was investigated by combined surface and thermal analysis. The progressive reduction of oxides was studied using model sintering cycles in hydrogen atmospheres in a thermogravimetric (TG) setup, with experiments ended at intermediate steps (500–1300°C) of the heating stage. The surface chemistry of the samples was then investigated by means of X‐ray photoelectron spectroscopy (XPS) to reveal changes that occurred during heating. The results show that reduction of the surface oxide layer occurs at relatively lower temperature for the steel powder, attributed to an influence of chromium, which is supported by a strong increase in Cr content immediately after oxide layer reduction. The reduction of the stable oxide particulates was shifted to higher temperatures, reflecting their higher thermodynamic stability. A complementary vacuum annealing treatment at 800°C was performed in a furnace directly connected to the XPS instrument allowing for sample transfer in vacuum. The results showed that Fe oxides were completely reduced, with segregation and growth of Cr and Mn oxides on the particle surfaces. This underlines the sequential reduction of oxides during sintering that reflects the thermodynamic stability and availability of oxide‐forming elements.
The paper examines the influence of carbon coating on iron nanopowder used as a sintering aid for water-atomized iron powder. Iron nanopowder without such a coating was used as a reference sintering aid to isolate the influence of the carbon coating. Both nanopowder variants were characterised using XPS and HRTEM. The results showed a core–shell structure for both variants. The iron nanopowder is covered by a 3–4 nm thick iron oxide layer, while the carbon-coated iron nanopowder is encapsulated with several nanometric carbon layers. Thermogravimetry conducted in a pure hydrogen environment shows a multipeak behaviour for the carbon-coated iron nanopowder, while a single peak behaviour is observed for the iron nanopowder. Two types of micro/nanobimodal powders were obtained by mixing the nanopowder with water-atomized iron powder. Improved linear shrinkage was observed during sintering when the carbon-coated iron nanopowder was added. This can be explained by the reduction in surface diffusion in the nanopowder caused by the carbon coating, which allows the nanopowder to sinter at higher temperatures and improves densification. Carbon and oxygen analysis, density measurements, optical microscopy and JMatPro calculations were also performed.