The use of polymeric materials such as geosynthetics in infrastructure works has been increasing over the last decades, as they bring down costs and provide long-term benefits. However, the aging of polymers raises the question of its long-term durability and for this reason researchers have been studying a sort of techniques to search for the required renewal time. This paper examined a commercial polypropylene (PP) nonwoven geotextile before and after 500 h and 1000 h exposure to ultraviolet (UV) light by performing laboratory accelerated ultraviolet-aging tests. The state of the polymeric material after UV exposure was studied through a wide set of tests, including mechanical and physical tests and thermoanalytical tests and scanning electron microscopy analysis. The calorimetric evaluations (DSC) showed distinct behaviors in sample melting points, attributed to the UV radiation effect on the aged samples. Furthermore, after exposure, the samples presented low thermal stability in the thermomechanical analysis (TMA), with a continuing decrease in their thicknesses. The tensile tests showed an increase in material stiffness after exposition. This study demonstrates that UV aging has effects on the properties of the polypropylene polymer.
High-density polyethylene (HDPE) geomembranes have been used for different applications in engineering including sanitation, such as landfills and waste liquid ponds. For these applications, the material can be exposed to aging mechanisms as thermal and chemical degradation, even to UV radiation and biological contact, which can degrade the geomembrane and decrease the material’s durability. This paper aims to present an experimental evaluation of two exhumed HDPE geomembranes, the first was used for 2.75 years in a sewage treatment aeration pond (LTE sample) and another was used for 5.17 years in a municipal landfill leachate pond (LCH sample). Physical and thermal analyses were used such as thermogravimetry (TG), differential thermal analysis (DTA), differential scanning calorimetry (DSC) and dynamic mechanic analysis (DMA). The thermogravimetric analyses showed significant changes in the LCH sample’s thermal decomposition probably caused by the interaction reactions between the polymer and the leachate. For the DSC analyses, the behavior seen in the LTE sample was not observed in the LCH sample. In the DMA analyses, the behavior of the LTE sample storage module shows which LCH sample is less brittle. The LTE sample presented low stress cracking resistance and low tensile elongation at break, following the DMA results.
High-density polyethylene (HDPE) geomembranes are polymeric geosynthetic materials usually applied as a liner in environmental facilities due to their good mechanical properties, good welding conditions, and excellent chemical resistance. A geomembrane’s field performance is affected by different conditions and exposures, including ultraviolet radiation, thermal and oxidative exposure, and chemical contact. This article presents an experimental study with a 1.0 mm-thick HDPE virgin geomembrane exposed by the Xenon arc weatherometer for 2160 h and the ultraviolet fluorescent weatherometer for 8760 h to understand the geomembrane’s behavior under ultraviolet exposure. The evaluation was performed using the melt flow index (MFI) test, oxidative-induction time (OIT) tests, tensile test, differential scanning calorimetry (DSC) analysis, and Fourier transform infrared spectroscopy (FTIR) analysis. The sample exposed in the Xenon arc equipment showed a tendency to increase the MFI values during the exposure time. This upward trend may indicate morphological changes in the polymer. The tensile behavior analysis showed a tendency of the sample to lose ductility, without showing brittle behavior. The samples’ OIT test results under both device exposures showed faster antioxidant depletion for the standard OIT test than the high-pressure OIT test. The DSC and FTIR analyses did not demonstrate the polymer’s changes.
High-density polyethylene (HDPE) water-proof membranes are used as coatings in vinasse (leachate from sugar cane) storage tanks. The leachate is pumped into the tanks at temperatures of 80-90 °C. Due to these high temperatures and acidity of the waste, these membranes can be degraded, cracked and then loose the function for which they have been designed. This may cause contamination of the soil and groundwater. This study evaluated the effect of vinasse in HDPE membranes after 4 months of exposure in a controlled environment. An aggressive, alkaline pH liquid (sodium hydroxide) was also used. The objective was to evaluate the membrane resistance in contact with acidic and alkaline residues. Physical and mechanical tests, measurement of the carbon black content and thermo gravimetric analysis (TGA) were used to determine degradation of polymer membranes after chemical immersion. While sodium hydroxide resulted caused only minor changes in the physical properties, vinasse induced a thickness change of 7.8%. With immersion in vinasse, an average decrease in strength and deformability (yield) of 34% and 23.5% were measured, respectively. The stiffness increased by 7.8% (average) and the tear strength decreased by 2.7% (average).Membranas impermeabilizantes de polietileno de alta densidade (PEAD) são utilizadas como revestimento em tanques de armazenamento de vinhaça (resíduo da cana-de-açúcar), onde esse resíduo é lançado a temperaturas médias de 80-90 °C. Devido a essas temperaturas elevadas e à acidez do resíduo, essas membranas podem degradar, fissurar e perder a função para a qual foram projetadas vindo a contaminar o solo e o lençol freático. Este trabalho avaliou o efeito da vinhaça em membranas de PEAD após 4 meses de exposição em ambiente controlado. De forma complementar, utilizou-se também um líquido agressivo de pH básico (soda cáustica). Objetivou-se avaliar a resistência da membrana em contato com esses resíduos (ácido e básico). Foram avaliadas as propriedades físicas, mecânicas, teor de negro de fumo e análise termogravimétrica (TGA) para quantificar a degradação das membranas poliméricas frente aos resíduos químicos utilizados. Os resultados mostram, por exemplo, que enquanto a soda cáustica provocou pequena variação nas propriedades físicas, a vinhaça alterou a espessura do material em 7,8%. Analisando-se a imersão na vinhaça, verificou-se uma diminuição média na resistência e deformabilidade (escoamento) de 34% e 23,5%, respectivamente. Houve um aumento médio na rigidez de 7,8% e uma pequena diminuição na resistência média ao rasgo (2,7%)