Prediction of the mechanical behavior of thin foils (~25 µm) requires special characterization techniques. The current work is focused on the mechanical and microstructural characterization of 25 µm HAVAR alloy foils following annealing, cold rolling, and subsequent heat treatments, using small punch testing (SPT), X-ray diffraction (XRD), and transmission-scanning electron microscopy (TEM). The SPT technique revealed that the annealed specimens exhibited the largest maximal load to failure and deformation (more than two-fold), compared to the cold rolled and heat treated conditions. The microscopy observations revealed high dislocation density following cold rolling and subsequent heat treatments. Following annealing, a cubic crystallographic structure (FCC) with equiaxed grains and a limited dislocation population was observed. Following cold rolling and subsequent thermal treatment, a preferred orientation texture (i.e., ‘deformation texture’) was observed with a very high dislocation density. The correlation between the mechanical behavior and the microstructural observations is discussed in detail.
The micro-structure of the spall plane of pure aluminum (99.9999%) was investigated in symmetric plate impact experiments. The aluminum targets were first heated at 450°C for 22 h for grain growth. The impacted targets were softly caught and collected for metallurgical analysis. It was found that at weak impacts with partial spall, voids with average size of 50±10 ìm were developed along the grain boundaries. The grain sizes in the vicinity of the voids are 50-250 μm, in comparison with grain sizes of 400-1000 μm in other areas of the specimen, revealing grains splitting under dynamic tension. Transmission Electron Microscopy (TEM) and electron diffraction show parallel dislocation walls, that create a sub-grain micro-structure inside grains with (011) orientation to the beam. In grains with other orientations no dislocation walls or sub-grain structure were found. We also found out pile up of the dislocations by glide mechanism along directions during the spall process.
The mechanical properties characterization of thin foils to be used as target in high intensity accelerator requires non standards techniques. Previous studies, focused on foils after annealed, cold rolled and heat treatment after rolled, in addition to foils at different thickness, have been carried out to estimate the sensitivity of the small punch test (SPT) technique in foils. In this research we studied the degradation of the mechanical properties of foils due to irradiation damage by high intensity proton beams. For this new study, two samples of SS316L foils have 25 μm thickness were exposed to proton bombardment at 3.6 MeV, and approximately 300 μA of current for a period of 3 hours and 40 hours, separately. The SPT technique revealed that the un-irradiated specimens exhibited the largest load and deformation before failure, rather than the irradiated foils. The electron microscopy observations (SEM) revealed high cross slips and pseudo-cleavage density combined with multiple deformation twinning after irradiation to high energy. The mechanical behavior can be explained by the microstructure. The crack propagation path is in a zigzag fracture mode when multiple deformation twinning occurs close to the stretched zone of the foil and failure. Changes of the SPT measurements were found and the degradation from ductile to brittle crack mode is attributed to radiation damage effects.