The paper is devoted to revealing the regularities of the influence of titanium (0.91, 2.42, 3.19, 3.39, 4.32 and 8.81 wt.%) on structure formation, nature of element distribution and microhardness of structural components in Al – Ni – Ti alloys by aluminothermy during SHS metallurgy. As the initial composition of the charge were selected the following materials in fractional parts: Al:NiO2:CaF2:NaNO3:TiO2 = 10:10:12:6:X, where X = 1.5, 4.5, 5.0, 7.0, 10.0. The structural components in Al – Ni – Ti alloys have been identified by electron microscopy and X-ray spectral analysis of elements. In the alloys with 0.91–4.32 wt.% Ti the following phases crystallize: β'-phase (solid solution of Ni in the nickel aluminide AlNi) Al3Ni2, Al3Ti, Al3Ni and α-solid solution of Ni and Ti in aluminum. In an alloy with 8.81 wt.% Ti the β'-phase turns into a titanium-doped nickel aluminide Al(NiTi) (composition in at.%: 50.53 Al; 1.47 Ti; 48.0 Ni). The increase of titanium content in Al – Ni – Ti alloys increases the solubility of Ni in the β'-phase and at titanium concentration in the alloy 8.81 wt.% in the aluminide Al(NiTi) up to 48 at.% Ni is dissolved compared to the solubility of nickel (38 at.%) in the alloy with 0.91 wt.% Ti. Increasing the nickel content in the above phases contributes to their microhardness from 13 GPa to 14.8 GPa at 8.81 wt.% Ti. Increasing the titanium content in Al – Ni – Ti alloys to 4.32 wt.% increases the solubility of nickel in the nickel aluminide Al3Ni, with a higher concentration of titanium (8.81 wt.%) in the nickel aluminide with titanium Al(NiTi) dissolves up to 48.53 at.% Ni, while in the alloy with 0.91 wt.% Ti – only about 1.0 at.% Ni. At the same time, the Al and Ti content in titanium aluminide Al3Ti decreases and its microhardness increases. It was not possible to determine the microhardness of Al(NiTi) aluminide because of the formation of a porous structure. In nickel aluminide Al3Ni, an increase in titanium content leads to an increase in nickel concentration to 4.32 wt.% Ti followed by a slight increase to 8.81 wt.% Ti. Despite increasing the nickel content and decreasing the aluminum concentration, the microhardness of the nickel aluminide decreases. Apparently, this circumstance is caused by the formation of a porous structure in this phase. The research was carried out at the Center for Collective Use “Applied Materials Science” of the Federal State Budgetary Educational Institution of Higher Education “TOGU” with the financial support of the Ministry of Science and Education of the Russian Federation within the framework of research work No state reg. of the state task AAAA-A20-120021490002-1.
Nickel aluminides of a composite structure, hardened by the inclusions of refractory transition metal compounds, have great potential in terms of creating new materials with the increased strength and heat resistance. The variety of compositions of alloying systems allows obtaining composite materials of different types with a complex of the improved operational characteristics. This work presents the research results of studying the synthesis conditions for metal matrix alloys from pure metal oxides. The microhardness, phase and element compositions of the resulting alloys have been investigated. It is found that composite alloys are formed in the result of thermally conjugated exothermic reactions in NiO – Al and WO3 – C – Al systems. Thermodynamic analysis shows that the probability of obtaining cast products in the result of such reactions is very high. The dominant reaction corresponds to the parameters: G = –944 kJ/mol, adiabatic temperature (AT = 3150 K. The influence of the synthesis conditions on the composition of the intermetallic phase of the composite has also been studied. The possibility of the formation of Ni2Al3 and NiAl intermetallic compounds is proved. It is established that in order to create optimal conditions for the formation of intermetallic compounds an excess amount of aluminum (~ 30 wt.%) in the total initial charge mixture is required. An increase of carbon in the composition of the initial charge mixture to ~ 20 wt.% raises the content of tungsten carbide in the synthesized alloy. In this case, a decrease in the temperature causes the formation of Ni2Al3 intermetallic phase. Composite materials are represented by NiAl and Ni2Al3 phases with WC tungsten carbide inclusions according to the results of elemental, X-ray phase analysis and scanning electron microscopy. The volumetric content of tungsten carbide in alloys is ~20%. The resulting alloys have the increased microhardness due to the inclusion of the refractory interstitial WC phase (8.5–9.8 GPa) in their structure. Composite materials based on NiAl are promising for application as heat-resistant coatings. The work was carried out within the project SP-1904.2019.1 “Development of an energy-saving technology for producing metal matrix composite materials from mineral concentrate (scheelite) for forming coatings with enhanced wear-resistant properties by ESA method on steel products” of the Federal Target Program “Scholarship of the President of the Russian Federation to young scientists and graduate students engaged in advanced research and development in priority areas of modernization of the Russian economy, for 2019–2021” with the financial support of the Ministry of Education and Science of the Russian Federation.
Using optical and electron scanning microscopy, as well as electron probe microanalysis and X-ray diffraction analysis, the authors looked at the structure, segregation and properties (hardness HRA, microhardness HV) of high-alloy Al – Ti – V – Ni alloys. It was established how the structure tends to change and how elements of the structural components of the studied alloys (1–5) tend to distribute as a function of V and Ni concentration. Using electron probe microanalysis, the structural conponents of the studied alloys were identified depending on V and Ni concentration. 1. The initial alloy 1 sees vanadium aluminide Al3(V, Ti) solidify from Al – Ti – V – Ni (wt. %: 24.6 V, 0 Ni), as well as alloyed vanadium carbide. The former solidifies as grey-coloured grains with a minimum size of 25 μm and serves as the base phase, whereas tha latter comes in a spiky shape (<25 μm). A blackish-coloured mixture of Al + Al3Ti + Al21V2 solidifies last. 2. Alloy 2 sees nickel aluminide Al3Ni solidify from Al – Ti – V – Ni (17 wt. % V, 7.2 wt. % Ni) as fine-grained light-coloured inclusions against a background of vanadium aluminate Al2(V, Ti), which is the key structural component of the alloy. Together with the above phases, alloyed titanium carbide (Al, Ti, V)3C forms in the alloy as compact grey-coloured grains. A phase mixture of Al + + Al3Ni + Al3Ti + Al21V2 solidifies last. 3. The following phases solidify in alloys 3–5 from Al – Ti – V – Ni (0–10.7 wt. % V; 13.5–23.8 wt. % Ni): β'-phase – a solid solution of Ni in nickel aluminide AlNi, which comes as fine-grained white-coloured inclusions against a background of nickel aluminide Al3Ni, which is the base phase. The next phase includes compact dark-grey grains of titanium carbide Ti2C. Alloys 4–5 see a new phase form – a complex alloyed titanium aluminide Al3(Ti, V, Ni), which consists of dark-grey oblong-shaped crystals. A phase mixture of Al + Al3Ni + Al3Ti + Al21V2 solidifies last. Even though the stoichiometry of the identified phases fails to match the results of electron probe microanalysis, the results of X-ray diffraction analysis confirms the presence of the key structural components in the studied alloys.This research was carried out using the equipment of the Applied Materials Science Centre at the Pacific National University. It was funded by the Ministry of Education and Science of the Russian Federation under Gove rnmental Assignment No. FEME-2020-0010.
Modern research on high-entropy alloys is aimed at studying the effect of composition and energy impacts on their microstructure and properties. The method of self-propagating high-temperature synthesis has advantages such as low cost, speed and simplicity compared to traditional methods for producing high-entropy alloys, however, in the absence of external influences, microdefects remain in the alloy structure. The energetic interaction of short-pulse electromagnetic fields with a strength of 105–107 V/m with a metallic liquid contributes to the destruction of its structure, increase of the solubility of modifying and alloying elements and the uniformity of their distribution. The purpose of this work was to study the effect of nanosecond electromagnetic pulses on the structure formation, hardness, and microhardness of the structural components of the Al – Ti – Cr – Ni – V – Zr system high–entropy alloys synthesized by self-propagating high-temperature synthesis. The structural components in the alloy of the Al – Ti – Cr – Ni – V – Zr system with nanosecond electromagnetic pulses amplitude from 0 to 40 kV have been identified by electron microscopy and element–phase analysis. It is determined that the structural components of this high-entropy alloy are complex-alloyed solid solutions of four types: a white solid solution, BCC(1) type solid solutions of light and dark gray colors, and a dark solid solution without zirconium. The amplitude dependence of the change in the content of elements in the structural components of the alloy of the Al – Ti – Cr – Ni – V – Zr system has been established. With an increase in the nanosecond electromagnetic pulses amplitude to 20 kV, the content of aluminum in the studied solid solutions of all types and of vanadium and chromium in solid solutions without zirconium increase significantly, and the concentrations of the remaining elements are practically independent of the nanosecond electromagnetic pulses amplitude. The maximum value of the microhardness of BCC(1) type solid solutions and a solid solution without zirconium is observed when irradiating a melt with nanosecond electromagnetic pulses with an amplitude of 20 kV.The study was conducted at the Shared Research Facility “Applied Materials Science” of the Pacific State University with the financial support of the Ministry of Science and Education of the Russian Federation within the framework of Research project No. AAAAA-A20-120021490002-1.
High-entropy alloys (HEA) have recently attracted widespread attention due to a new metallurgical approach to the development of alloys. Meanwhile, the problem that hinders the economical production of these alloys is the expensive metal raw materials and high energy costs in vacuum arc melting, which is the most commonly used production method (according to literature sources). To solve this problem, the self-propagating high-temperature synthesis (SHS) method stands out as a potentially inexpensive, fast and simple one. There are several studies on the production of HEA by the SHS method for the AlxCoCrFeNi, CoCrFeNiMn, NiCrCoFeMnAlx and AlCoCrFeNiMe (Me = B, Cu, Ti) alloy systems. The presented work is devoted to establishing the pattern of the influence of zirconium and vanadium additives on the structure formation and properties in the Al – Ti – Cr – Ni – VхZr1-х alloys obtained by aluminothermy using SHS metallurgy. Using optical and electron microscopy, X-ray microprobe and X-ray diffraction analysis, the features of structure formation and liquation processes in the structural components of high-entropy alloys of the Al – Ti – Cr – Ni – VхZr1–х system synthesized by SHS metallurgy were studied. The patterns of changes in the structure and element distribution behavior in the studied alloys were revealed depending on the addition of zirconium and vanadium. It was found that vanadium additions make it possible to homogenize thermite mixtures and obtain a uniform structure in high-entropy alloys of the Al – Co – Cr – Fe – Ni system synthesized by SHS metallurgy. The presence of the main structural components in the studied alloys was confirmed by the results of X-ray diffraction analysis, although the stoichiometry of the identified phases does not coincide with the X-ray microprobe analysis results. The dependence of the effect of additives on the microhardness of the structural components was established.The research was conducted at the Center for Collective Use “Applied Materials Science” of the FSBEI HE “PNU” with the financial support of the Ministry of Science and Education of the Russian Federation within the framework of R&D of state assignment No. AAAA-A20-120021490002-1.