The authors review the methods of dust emission suppression at operated and abandoned tailings storages. The environmental impact of mineral dust particles and the after-effects are greatly varied. Dust suppression in surface layer of tailings ponds can use the most widely applied chemical methods, as well as mechanical and biological methods. The requirements imposed on binding agents are efficiency, dust catching, longevity and the environmental safety. Dust suppression control can utilize natural climatic events, e.g., seasonal freezing–thawing of tailing surface. The described engineering solutions concern techniques and equipment for spreading suitable chemical agents for dust suppression at overburden dumps and tailing storage facilities at mining and processing plants.
The possibility of applying a combined concentration and metallurgical method for processing low-grade and refractory copper–nickel ores was considered. The resulting rougher and scavenger flotation concentrate contained 2.07% nickel and 0.881% copper at a recovery of 85.44% and 89.91%, respectively. The concentrate was then roasted with ammonium sulfate, followed by aqueous leaching of clinker to dissolve nickel and copper. The roasting temperature, the ratio of concentrate to (NH4)2SO4 in the mixture, and the temperature were varied. Based on the study findings, the following process conditions were found to be optimal: roasting temperature 400 °C, rougher concentrate to ammonium sulfate ratio 1:7, and grinding size −40 μm. A roasting temperature of 400 °C is significantly lower than the temperature applied in conventional pyrometallurgical processes. The possibility of collecting off-gases allows the reagent to be regenerated and makes the process even more cost-effective. End-to-end recovery into pregnant solution was 81.42% for nickel and 82.81% for copper. The resulting solutions can be processed by known hydrometallurgical methods.
The goal of the present work was to study the recovery of copper, nickel, and platinum group metals (PGMs) (Pt and Pd) from low-grade copper–nickel ore containing pyrrhotite, pentlandite, and chalcopyrite by column bioleaching followed by cyanidation. The ore sample contained the following: Ni—0.74%, Cu—0.23%, Fe—14.8%, Stotal—8.1%, and Ssulfide—7.8%. The Pt and Pd contents in the ore sample were 0.2535 and 0.515 g/t, respectively. Biological leaching in columns was carried out at 25, 35, and 45 °C for 140 days. A mixed culture of acidophilic microorganisms was used as an inoculum. Cu and Ni extraction depended on temperature, and at 45 °C, copper and nickel recovery was the highest, being 2.1 and 1.8 times higher than that at 25 °C, respectively. As a result, up to 35% of nickel and up to 10% of copper were recovered by bioleaching within 140 days. Bioleaching resulted in an increase in Pt and Pd recovery by cyanidation, but the effect on Pd recovery was insignificant. Pt recovery varied in the range of 3–40% depending on process conditions; Pd recovery was 44–55%.
The feasibility of processing low-grade copper-nickel ores by heap bioleaching was investigated. It was found that an iron-oxidizing strain of acidophilic microorganisms, Acidithiobacillus ferrivorans, is effective in the leaching of sulfide ores from the deposits in Russia’s Murmansk region. Sulfide mineralization of the studied mineral feeds was described using the methods of X-ray phase analysis and optical microscopy. In the process of leaching, the pH and Eh values and the concentrations of ferric and ferrous iron, nickel, and copper ions were monitored. By the end of the experiment, 16.5% of nickel and 7.5% of copper was recovered from the ore of the Allarechensk technogenic deposit, while 22.5% of nickel and 12.7% copper were recovered from the ore of the Nud II deposit. By silicate analysis of the solid phase, patterns of ore chemistry change were described during the process of bioleaching.
A laboratory scale study was conducted, aimed at finding an effective method for processing fine concentration tailings of copper-nickel ores. A sulfuric acid tailing granulation process followed by subsequent heap leaching of granules is proposed. Various methods of preparation and storage of the granular material are discussed. A solution of sulfuric acid was used as a binder. It was found that the addition of an oxidizing agent (Fe3+ and NO2−) when irrigating the granules had an effect on the recovery of metals. Changes in the recovery performance of non-ferrous metals into solution were studied under subsequent heap leaching of the material during a period of positive temperatures. The role of nitrogen compounds, in particular, nitrous acid, on the recovery of metals into solution after the preliminary storage of granules at below 0 °C temperatures is also discussed.
The phase transitions of sulfide minerals—pentlandite and chalcopyrite—are tested in roasting with mixture with ammonium sulfate. The behavior of the mixture during roasting is assessed via the synchronous thermal and X-ray phase analyses, and by scanning electron microscopy. The basic optimal technology parameters for the efficient processing of sulfide-bearing copper–nickel ore are selected to be: the roasting temperature of 400 °C, the ore: ammonium sulfate ratio of 1:10, the particle size of –40 \(\mu\)m and the roasting time of 240 min. An important condition is joint milling of ore and ammonium sulfate down to the specified size. Given these parameters, the later on water leaching of clinker provided extraction of 94.8% of copper, 91.5% of nickel and 82.3% of cobalt. The research findings are of essential practical interest owing to the high recovery of the target minerals.