Synthesis of nanosized particle of Ag-doped hydroxyapatite with antibacterial properties is in the great interest in the development of new biomedical applications. In this article, we propose a method for synthesized the Ag-doped nanocrystalline hydroxyapatite. A silver-doped nanocrystalline hydroxyapatite was synthesized at 100°C in deionized water. Other phase or impurities were not observed. Silver-doped hydroxyapatite nanoparticles (Ag:HAp) were performed by setting the atomic ratio of Ag/[Ag + Ca] at 20% and [Ca + Ag]/P as 1.67. The X-ray diffraction studies demonstrate that powders made by co-precipitation at 100°C exhibit the apatite characteristics with good crystal structure and no new phase or impurity is found. The scanning electron microscopy (SEM) observations suggest that these materials present a little different morphology, which reveals a homogeneous aspect of the synthesized particles for all samples. The presence of calcium (Ca), phosphor (P), oxygen (O), and silver (Ag) in the Ag:HAp is confirmed by energy dispersive X-ray (EDAX) analysis. FT-IR and FT-Raman spectroscopies revealed that the presence of the various vibrational modes corresponds to phosphates and hydroxyl groups. The strain of Staphylococcus aureus was used to evaluate the antibacterial activity of the Ca10-xAgx(PO4)6(OH)2 (x = 0 and 0.2). In vitro bacterial adhesion study indicated a significant difference between HAp (x = 0) and Ag:HAp (x = 0.2). The Ag:Hap nanopowder showed higher inhibition.
Magnesium-doped hydroxyapatite/chitosan composite coatings produced by the radio-frequency magnetron sputtering technique were exposed to 5 MeV electron beams of 8 and 30 Gy radiation doses in a linear electron accelerator. The surfaces of unirradiated layers are smooth, while the irradiated ones exhibit nano-structures with sizes that increase from 60 nm at a 8 Gy dose to 200 nm at a 30 Gy dose. Young’s modulus and the stiffness of the layers decrease from 58.9 GPa and 10 µN/nm to 5 GPa and 2.2 µN/nm, respectively, when the radiation doses are increased from 0 to 30 Gy. These data suggest the diminishing of the contribution of the chitosan to the elasticity of the magnesium-doped hydroxyapatite/chitosan composite layers after electron beam irradiation. The biological capabilities of the coatings were assessed before and after their immersion in RPMI-1640 cell culture medium for 7 and 14 days, respectively, and further cultured with a MG63 cell line (ATCC CRL1427) in Dulbecco’s Modified Eagle Medium supplemented with fetal bovine serum, penicillin–streptomycin, and L-glutamine. Thus, 1 µm spherical structures were developed on the surfaces of the layers exposed to a 30 Gy radiation dose and immersed for 14 days in the RPMI-1640 biological medium. The molecular structures of all the RPMI-1640 immersed samples were modified by the growth of a carbonated hydroxyapatite layer characterized by a B-type substitution, as Fourier Transform Infrared Spectroscopy revealed. The biological assay proved the increased biocompatibility of the layers kept in RPMI-1640 medium and enhanced MG63 cell attachment and proliferation. Atomic force microscopy analysis indicated the elongated fibroblastic cell morphology of MG63 cells with minor alteration at 30 Gy irradiation doses as a result of layer biocompatibility modifications.