Alloy 825 is a nickel-based alloy that is commonly used in applications where both high strength and corrosion resistance are required, such as tanks in the chemical, food and petrochemical industries and oil and gas pipelines. Components made from Alloy 825 are often manufactured using hot deformation. However, there is no systematic study to optimise the processing conditions reported in literature. In this study, a processing map for as-cast Alloy 825 is established to maximise the power dissipation efficiency of hot deformation in the temperature range of 950 to 1250 °C at an interval of 50 °C and strain rate range of $$0.01\, {\text{s}}^{ - 1}$$ to $$10.0\, {\text{s}}^{ - 1}$$ to a true strain of $$0.7$$ using a Gleeble-3500 thermomechanical simulator. The processing conditions are also correlated to the Vickers hardness of the final material, which is also characterised using optical microscopy and scanning electron microscopy, including electron backscattered diffraction. The true stress-true strain curves exhibit peak stresses followed by softening due to occurrence of dynamic recrystallization. The activation energy for plastic flow in the temperature range tested is approximately $$450\,{\text{ kJ mol}}^{ - 1}$$ , and the value of the stress exponent in the (hyperbolic sine-based) constitutive equation, $$n = 5.0$$ , suggests that the rate-limiting mechanism of deformation is dislocation climb. Increasing deformation temperature led to a lower Vickers hardness in the deformed material, due to increased dynamic recrystallization. Raising the strain rate led to an increase in Vickers hardness in the deformed material due to increased work hardening. The maximum power dissipation efficiency is over $$35\%$$ , obtained for deformation in the temperature range 1100-1250 °C and a strain rate of $$0.01\, {\text{s}}^{ - 1}$$ - $$0.1\, {\text{s}}^{ - 1}$$ . These are the optimum conditions for hot working.
Wrought nickel-based Alloy 825 is widely used in the oil and gas industries, attributed to its high strength at temperatures up to 540 °C. However, differences in mechanical properties arise in finished components due to variations in both grain size and dislocation density. Numerous experimental studies of the strengthening mechanisms have been reported and many models have been developed to predict strengthening under thermomechanical processing. However, there are debates surrounding some fundamental issues in modeling and the interpretation of experimental observations. Therefore, it is important to understand the evolution of strain within the material during the hot-forging process. In addition, there is a lack of research around the behavior during hot deformation and subsequent stabilization of Alloy 825. This article investigates the origin of this strength and considers a variety of strengthening mechanisms, resulting in a quantitative prediction of the contribution of each mechanism. The alloy is processed with a total forging strain of 0.45, 0.65, or 0.9, and subsequent annealing at a temperature of 950 °C, reflecting commercial practice. The microstructure after annealing is similar to that before annealing, suggesting that static recovery is dominant at this temperature. The maximum yield strength and ultimate tensile strength were 348 MPa and 618 MPa, respectively, obtained after forging to a true strain of 0.9, with a ductility of 40%. The majority of strengthening was attributed to grain refinement, the dislocation densities that arise due to the large forging strain deformation, and solid solution strengthening. Precipitate strengthening was also quantified using the Brown and Ham modification of the Orowan bowing model. The results of yield strength calculations are in excellent agreement with experimental data, with less than 1% difference. The interfacial energy of Ti(C,N) in the face-centered cubic matrix of the current alloy has been assessed for the first time, with a value of 0.8 mJm−2. These results can be used by future researchers and industry to predict the strength of Alloy 825 and similar alloys, especially after hot-forging.
Hot-compression tests down to 0.7 in nominal strain were conducted at a strain rate of 1s-1 between 800 and 1200 °C. The material was taken from the columnar and equiaxed zones of a continuous cast strand of Alloy 825. Furthermore, recrystallization was determined using LOM and FEG-SEM equipped with an EBSD-detector. The true stress of the columnar structure was a 0.2% lower than for the equiaxed microstructure for the studied deformation temperatures. The optical and EBSD images in both structures showed that a dynamic recrystallization had almost not occurred. Instead, a substructure formation with mostly low-angle grain boundaries dominated was found.
Alloy 825 is widely used in several industries, but its useful service life is limited by both mechanical properties and corrosion resistance. The current work explores the effect of the addition of magnesium on the recrystallization and mechanical behavior of alloy 825 under hot compression. Compression tests were performed under conditions representative of typical forming processes: temperatures between 1100 and 1250 °C and at strain rates of 0.1–10 s−1 to a true strain of 0.7. Microstructural evolution was characterized by electron backscattered diffraction. Dynamic recrystallization was found to be more prevalent under all test conditions in samples containing magnesium, but not in all cases of conventional alloy 825. The texture direction was the dominant orientation parallel to the longitudinal direction of casting (also the direction in which the samples were compressed) in samples that contained magnesium under all test conditions, but not in any sample that did not contain magnesium. For all deformation conditions, the peak stress was approximately 10% lower in material with the addition of magnesium. Furthermore, the differences in the peak strain between different temperatures are approximately 85% smaller if magnesium is present. The average activation energy for hot deformation was calculated to be with the addition of magnesium and without magnesium. The average size of dynamically recrystallized grains in both alloys showed a power law relation with the Zener–Hollomon parameter, , and the exponent of value, , is found to be . These results can be used to design optimized compositions and thermomechanical treatments of alloy 825 to maximize the useful service life under current service conditions. No experiments were conducted to investigate the effects of such changes on the service life and such experiments should now be performed.