The microstructure of the Si phase in Al-20Si alloys solidified under high pressure was investigated. The results demonstrate that the morphology of Si phase transformed (bulk→short rod→long needle) with the increase of superheat temperature under high pressure. At a pressure of 3 GPa and a superheat temperature of 100 K, a microstructure with a uniform distribution of fine Si phases on the α-Al matrix was obtained in the Al-20Si alloy. In addition, a mathematical model was developed to analyze the spacing variation of the lamellar Al-Si eutectics under the effect of pressure. The lamellar Al-Si eutectics appeared at 2 GPa and superheat temperatures of 70–150 K, and at 3 GPa and superheat temperatures of 140–200 K. With the increase of pressure from 2 GPa to 3 GPa, the average spacing of lamellar Al-Si eutectics decreased from 1.2–1.6 μm to 0.9–1.1 μm. In binary alloys, the effect of pressure on the eutectic spacing is related to the volume change of the solute phase from liquid to solid. When the volume change of the solute phase from liquid to solid is negative, the lamellar eutectic spacing decreases with increasing pressure. When it is positive, the eutectic spacing increases with increasing pressure.
The microstructure and mechanical properties of SiC/Al-40Si composites prepared under high pressure were studied. As the pressure increases from 1 atm to 3 GPa, the primary Si phase in the Al-40Si alloy is refined. With increasing pressure, the composition of the eutectic point increases, the solute diffusion coefficient decreases exponentially, and the concentration of Si solute at the front of the solid–liquid interface of the primary Si is low, which contributes to the refining of the primary Si and inhibiting its faceted growth. The bending strength of SiC/Al-40Si composite prepared under 3 GPa was 334 MPa, which was 66% higher compared to the Al-40Si alloy prepared under the same pressure.
The formation of coarse primary Si is the main scientific challenge faced in the preparation of high-Si Al matrix composites. The SiC/Al-50Si composites are prepared by high pressure solidification, which allows the primary Si to form a SiC–Si spherical microstructure with SiC, while the solubility of Si in Al is increased by high pressure to reduce the proportion of primary Si, thus enhancing the strength of the composites. The results show that the high melt viscosity under high pressure makes the SiC particles almost “fixed” in situ. The SEM analysis shows that the presence of SiC in the growth front of the primary Si will hinder its continued growth and eventually form SiC–Si spherical microstructure. Through aging treatment, a large number of dispersed nanoscale Si phases are precipitated in the α-Al supersaturated solid solution. The TEM analysis shows that a semi-coherent interface is formed between the α-Al matrix and the nanoscale Si precipitates. The three-point bending tests shows that the bending strength of the aged SiC/Al-50Si composites prepared at 3 GPa is 387.6 MPa, which is 18.6% higher than that of the unaged composites.
The microstructures of Mg-1Sn-2.5Y (wt%) alloys solidified under high pressures were investigated. In addition, a mathematical model was established to analyze the effects of solidification pressure and cooling rate on the average grain size. The results show that the alloy was solidified under high pressure and temperature gradient using the cooling rate difference in the high pressure chamber, resulting in the formation of the outer equiaxed zone, the columnar zone, and the equiaxed zone in the sample. With an increase in the solidification pressure, the columnar-to-equiaxed transition was inhibited in Mg-1Sn-2.5Y alloy. In the outer fine equiaxed zone and the columnar zone, the solubility of Sn in the Mg matrix increased with an increase in solidification pressure. The average secondary dendrite arm spacing decreased from 14–17 μm under 1 GPa to 9–11 μm under 1.5 GPa. Increases in pressure and cooling rate resulted in a reduction in average grain size.
First-principles calculations based on density functional theory (DFT) are performed to investigate the interfacial properties and fracture behavior of 3C-SiC(111)/Al(111) and 4H-SiC(0001)/Al(111) interfaces. To mitigate surface effects through adequate slab thickness, the interface models are constructed by positioning a seven-layer Al(111) slab atop eight-layer 3C-SiC(111) and 14-layer 4H-SiC(0001) slabs, respectively. Accounting for the distinct surface terminations and stacking sequences of each polytype, six interface configurations are established: C-top, -center, and -hollow; Si-top, -center, and -hollow. Based on the simulation results of surface energy, work of separation, and electron density distribution, the C-top configuration yields the most stable SiC/Al interface structure, exhibiting the highest work of separation. The ultimate tensile strengths of the C-top interfaces are 6.603 GPa (3C-SiC/Al) and 6.851 GPa (4H-SiC/Al), with corresponding tensile strains of 10% and 12%, respectively. Tensile fracture initiates exclusively within the Al slab for all C-top interfaces, but at distinct atomic layers: fracture occurs between the second and third Al layers (Al2–Al3) for 3C-SiC/Al; and between the first and second Al layers (Al1–Al2) for 4H-SiC/Al. This distinction reflects the influence of different interfacial configurations on the bonding strength between aluminum atomic layers. In summary, an atomic-scale investigation of the interfacial properties and fracture behavior of SiC/Al interfaces provides critical insights for the design and fabrication of novel ceramic/metal composites.