Soda-ethanol pulps, prepared from a forestry residue pine sawdust, were treated according to high-consistency enzymatic fibrillation technology to manufacture nanocellulose. The obtained nanocellulose was characterized and used as ink for three-dimensional (3D) printing of various structures. It was also tested for its moisture sorption capacity and cytotoxicity, as preliminary tests for evaluating its suitability for wound dressing and similar applications. During the high-consistency enzymatic treatment it was found that only the treatment of the O2-delignified pine pulp resulted in fibrillation into nano-scale. For 3D printing trials, the material needed to be fluidized further. By 3D printing, it was possible to fabricate various structures from the high-consistency enzymatic nanocellulose. However, the water sorption capacity of the structures was lower than previously seen with porous nanocellulose structures, indicating that further optimization of the material is needed. The material was found not to be cytotoxic, thus showing potential as material, e.g., for wound dressings and for printing tissue models.
The soda–ethanol process was conceived as a sulfur-free pulping process, which may also be an alternative to conventional alkaline pulping, such as kraft or soda–AQ in the biorefinery context. An in-depth study using two experimental designs was conducted to establish the viability of soda–ethanol delignification of pine sawdust. At first, a simple factorial design involving the ethanol–water ratio (ethanol:water) and the alkaline load (AL, % over dry wood, odw) was applied to define the levels of these variables and their eventual interaction. Then, a 32 experimental design was performed to evaluate the ability of the process concerning the pulping of pine sawdust. The tested conditions were carefully selected to screen a broad range of cooking times (60, 100, and 140 min) and alkaline loads (19.0, 23.3, and 27.6 %odw) to obtain pulps with different extents of delignification (residual lignin contents). Finally, the kraft, soda–AQ, and soda–ethanol treatments were compared. Soda–ethanol pulping was shown to be a suitable delignification stage for a biorefinery scheme of Pinus elliottii and Pinus taeda sawdust. It has many advantages over traditional processes regarding its environmental impact, harmless chemicals, and selectivity. The tested conditions were similar to those frequently used in conventional pulping at an industrial scale, suggesting the technical feasibility of the soda–ethanol process for pine sawdust processing.
This work proposes a sequential combination of steam explosion and organosolv delignification for Pinus radiata fractionation. An efficient pretreatment to fully optimize the use of lignocellulosic materials is the key to make a biorefinery profitable, especially for softwoods, known to be more recalcitrant than other lignocellulosic raw materials. Steam explosion has a dual effect on biomass as morphological and chemical changes are introduced. A delignifying stage has been stated to be necessary in order to ease hydrolytic enzymes accessibility to cellulose while avoiding non-productive bonds with the lignin present. Three steam explosion conditions were tested (170°C, 5 min; 180°C, 10 min; 170°C, 5+5 min) followed by an organosolv delignification stage, carried out at two different conditions (170°C, 60 min; 170°C, 90 min). All treatment yields, delignification extent, and hydrolysis yields were determined to evaluate each stage. The steam explosion treatment did not produce high delignification extent. Maximum global delignification (50,4%) was achieved when combining the two-cycle steam explosion with the most severe post-treatment condition tested. Enzymatic hydrolysis of the cellulosic residue improved after organosolv delignification; however, hydrolysis yields did not exceed 35%. The chemical changes undergone by softwood lignins are presumably responsible for the low digestibility.