() thin films having a thickness of several nanometers and showing both strong perpendicular magnetic anisotropy (PMA) and low magnetic damping are reported. The films are deposited by magnetron sputtering at room temperature first and then annealed in at high temperature. The substrates are , which share the same crystalline structure as , but have a lattice constant slightly larger than that of ; the lattice mismatching gives rise to an out-of-plane compressive strain and PMA in the films. The PMA is confirmed by vibrating sample magnetometer, magneto-optical Kerr effect, anomalous Hall effect, and angle-dependent ferromagnetic resonance (FMR) measurements. The damping of the films is analyzed through frequency-dependent FMR measurements. As an example, an 8-nm-thick film shows an effective PMA field of about 2800 Oe, a nearly square hysteresis loop, and a damping constant of only . As an illustration of possible applications of such films in spintronic devices, current-induced switching of the magnetization of the PMA films is demonstrated by the use of / bilayered Hall bar devices.
This letter reports the development of low-damping yttrium iron garnet (YIG) thin films via sputtering. The films were deposited by sputtering at room temperature first and were then annealed in O $_2$ at high temperature. It is found that the annealing temperature critically affects the structural properties of the YIG films and thereby dictates the static and dynamic properties of the films. A 75-nm-thick YIG film annealed at 900 °C shows a rms surface roughness of 0.08 nm, a coercivity of only 14 A/m (or 0.18 Oe), a saturation induction of 0.1778 T (or 1778 G) which is very close to the bulk value, a gyromagnetic ratio of 2.82×10 $-4$ MHz/T (or 2.82 MHz/Oe) which almost matches the standard value, and a Gilbert damping constant of α ∽ 5.2×10 $_5$ which is the lowest among the values reported so far for magnetic films in the nanometer thickness range. Frequency-dependent ferromagnetic resonance measurements with different field orientations confirmed that two-magnon scattering, if present, is very weak, and the measured damping value represents the actual damping of the YIG film.
The role of damping in the spin Seebeck effect (SSE) was studied experimentally for the first time. The experiments used Y3Fe5O12 (YIG)/Pt bilayered structures where the YIG films exhibit very similar structural and static magnetic properties but very different damping. The data show that a decrease in the damping gives rise to an increase in the SSE coefficient, which is qualitatively consistent with some of the theoretical models. This response also shows quasi-linear behavior, which was not predicted explicitly by previous studies. The data also indicate that the SSE coefficient shows no notable correlations with the enhanced damping due to spin pumping, which can be understood in the frame of two existing models.
Spin pumping is a technique widely used to generate pure spin current and characterize the spin-charge conversion efficiency of heavy metals. Upon microwave excitation, the sample may also be heated, and the parasitic thermoelectric signals could contaminate the spin pumping results. Owing to their identical angular dependences with respect to the magnetic field, it is difficult to isolate one from the other. In this paper, we present a quantitative method to separate thermoelectric contributions from spin pumping signals in both and bilayers through microwave photoresistance measurements. We find that the microwave absorption indeed can raise the temperature of samples, resulting a field-dependent thermoelectric hysteresis loop. However, the additional heat dissipation due to the resonant precession of the magnetization in the ferromagnet is negligibly small compared with the measured spin pumping signal. Thus, we conclude that the spin pumping signal is free of any detectable thermoelectric contributions.