The preparation of Ni-Mn-Ga and Ni-Mn-Ga-Fe master alloy ingots and microwires was completed by high vacuum electric furnace melt melting furnace and melt drawing liquid forming equipment, and the lattice dislocations and defects formed inside the microwires during the preparation process were corrected by stepwise ordered heat treatment. The micro-structure and phase structure were characterized using a SEM field emission scanning electron microscopy and an XRD diffractometer combined with an EDS energy spectrum analyzer; the martensitic phase transformation process of the microwires was analyzed using a DSC differential scanning calorimeter; and the superelasticity of the microwires was tested by a Q800 dynamic mechanical analyzer. The results indicate that Fe doping can refine the grain, transform the phase structure from parent phase to single 7M martensite, reduce the number of martensitic variants, and increase the mobility of the twin grain boundary interface. The MT phase transition temperature (MS) is substantially increased in the martensite transition (MT) process by the increase of the number of free electrons in its lattice. During the superelasticity (SE) test, both microwires displayed superior recover-ability of SE curves, and the Fe doping curves showed similar characteristics of “linear superelasticity”, showing higher critical stress values and complete SE in the experiment. The critical stress satisfies the Clausius-Clapeyron equation and exhibits higher temperature sensitivity than Ni-Mn-Ga microwires.
Ni50Mn25Ga20Fe5 ferromagnetic shape memory alloy microwires with diameters of ∼ 30–50 μm and grain sizes of ∼ 2–5 μm were prepared by melt-extraction technique. A step-wise chemical ordering annealing was carried out to improve the superelasticity strain and recovery ratio which were hampered by the internal stress, compositional inhomogeneity, and high-density defects in the as-extracted Ni50Mn25Ga20Fe5 microwires. The annealed microwires exhibited enhanced atomic ordering degree, narrow thermal hysteresis, and high saturation magnetization under a low magnetic field. As a result, the annealed microwire showed decreased superelastic critical stress, improved reversibility, and a high superelastic strain (1.9%) with a large recovery ratio (> 96%). This kind of filamentous material with superior superelastic effects may be promising materials for minor-devices.
The shape memory capabilities of Heusler alloy microwires with two different contents of Fe element instead of Ga element following step-by-step ordering heat treatment were explored based on the stoichiometric ratio of Ni2MnGa. The melt-drawing technique was used to create the polycrystalline microwires, and the two microwires had Fe atomic contents of 4.7 at.% and 5.5 at.%, respectively. The field emission scanning electron microscope was used to analyze the microwire’s surface condition as well as the microscopic tensile fracture morphology. Using an X-ray diffractometer, the microwires’ crystal structure was identified for phase analysis. Differential scanning calorimetry was used to examine the microwires’ behavior during martensitic transformation. Using a dynamic mechanical stretcher, the elongation and recovery rate of microwires’ one- and two-way shape memory behavior were examined. The findings demonstrated that the microwire phase structure, martensitic transformation behavior, and shape memory capabilities all displayed good properties after the heat treatment was ordered.