One of the most widely used materials for the fabrication of prosthetic dental parts is acrylic resin. Its reasonable mechanical and physical properties make it a popular material for a wide range of dental applications. Recently, many attempts have been made to improve the mechanical and biological properties of this material, such as by adding fibres, nanoparticles, and nanotubes. The current study aimed to evaluate the effects of adding an antimicrobial agent, Ag-Zn zeolite, on the surface roughness and hardness of the denture base resins. Ag-Zn zeolite particles were chemically prepared and added at different concentrations (0.50 wt.% and 0.75 wt.%) to the heat cure (HC) and cold cure (CC) acrylic resins. Zeolite particles were characterized and confirmed using X-ray diffraction (XRD) and Energy-Dispersive X-ray Spectroscopy (EDX) attached with a Scanning Electron Microscope (SEM). Sixty disk shape specimens (40 mm diameter and 2 mm thickness) were fabricated from the HC and CC resins with and without the zeolite. All the specimens were divided into two main groups based on the acrylic resins, then each was subdivided into three groups (n = 10) according to the concentration of the Ag-Zn zeolite. A surface roughness and a hardness tester were used to measure the surface finish and hardness of the specimens. The analysed data showed that the surface roughness values significantly decreased when 0.50 wt.% and 0.75 wt.% zeolite were incorporated in the HC resin specimens compared to the control group. However, this reduction was not significant in the case of CC resin, while the surface hardness was significantly improved after incorporating 0.50 wt.% and 0.75 wt.% zeolite for both the CC and HC resins. Incorporating Ag-Zn zeolite with acrylic resin materials could be beneficial for improving their surface finish and resistance to surface damage as defined by the higher hardness.
Aim: The paper aimed to evaluate using a modified flask on surface hardness and roughness, flexural, and tensile strength for heat-polymerized acrylic resin. Materials and methods: 80 specimens of heat-polymerized acrylic resin were prepared, and divided into two main groups. This division was followed type of flask that was used for processing the acrylic. 40 specimens of the first group (control) were prepared using a regular flasking technique, and the remaining 40 specimens were prepared using a modified flask which represented a second (testing) group. Then each group subdivided into another four groups according to the test will be done (10 specimens for each test group) hardness, flexural strength, tensile strength, and surface roughness, a statistical analysis with a p-value ≤ 0.05 was carried out for values obtained. Results: The amount of surface hardness (shore D) were 33.14 ± 2.04 and 29.57 ± 1.23; the flexural strengths (MPa) were 107.3 ± 9.54 and 89.92 ± 2.05; the tensile strengths (MPa) were 31.30 ± 8.46 and 15.50 ± 2.46; and surface roughness (μm) values were 1.15 ± 0.556 and 0.78 ± 0.29 for the experimental and control groups, respectively. There were noticeable effects on surface hardness, flexural and tensile strength with p-value < 0.05, and unnoticeable effects on surface roughness when compared between experimental and control groups. Conclusion: According to the result of this study, the mechanical properties of heat-polymerized acrylic resin were improved using a modified flask with a new metal plate.